Titanium carbide reinforced nickel tungsten powder, preparation method and application
Through vacuum smelting, atomization and heat treatment methods, diffusion-enhanced nickel tungsten powder was prepared, which solved the problems of high particle size requirements of titanium carbide and many powder defects in the prior art, and achieved high performance preparation of nickel tungsten alloys.
Patent Information
- Application Number
- CN202411068979.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-06
AI Technical Summary
In the prior art, when preparing titanium carbide reinforced metal cermet powder, the particle size of the titanium carbide particles is fine and costly, and there are many internal defects in the powder, which affects the performance of additive manufacturing alloys.
Through vacuum smelting, atomization and heat treatment methods, metallurgical combination of titanium carbide and nickel tungsten matrix is formed, and the replacement reaction between titanium carbide and titanium is used to prepare titanium carbide diffusion-strengthening nickel tungsten powder, reducing raw material particle size requirements and reducing powder defects .
A small size and few defects are obtained, which improves the density and performance of the alloy, and is suitable for laser cladding to prepare high-performance titanium carbide diffused reinforced nickel tungsten alloy.
Smart Images

Figure CN118976903A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additive manufacturing, and in particular to titanium carbide reinforced nickel-tungsten powder, a preparation method and application thereof. Background Art
[0002] Metal ceramics are widely used in aerospace, petrochemical, automobile and shipbuilding industries due to their high toughness, high hardness and high wear resistance. The most common metal ceramic is cobalt-tungsten carbide, which has high wear resistance and good economic applicability, among which tungsten carbide plays a key role as a wear-resistant phase. However, tungsten carbide is easily oxidized and decomposed when the temperature exceeds 800°C, resulting in a significant decrease in the performance of metal ceramic materials such as stability.
[0003] Compared with tungsten carbide, titanium carbide has better high temperature resistance and oxidation resistance, and is used in the preparation of new metal ceramic materials. However, the current preparation of metal ceramic powder containing titanium carbide generally adopts the direct composite granulation method of metal powder and titanium carbide powder. On the one hand, this method requires that the particle size of titanium carbide raw material particles is very fine, generally requiring the titanium carbide particle size to be less than 1 micron, but titanium carbide itself has high hardness and is not easy to break, resulting in difficult processing of raw materials and high costs; on the other hand, after the composite granulation of metal and titanium carbide powder, the internal defects of the powder are high, and the two are not easy to form a metallurgical bond, and the powder performance is poor, which affects the performance of subsequent additive manufacturing alloy preparation.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a titanium carbide reinforced nickel-tungsten powder, a preparation method and an application thereof, and to provide a powder with few internal defects.
[0006] The present invention is achieved in that:
[0007] In a first aspect, the present invention provides a titanium carbide reinforced nickel-tungsten powder, comprising a nickel-tungsten composite matrix and a titanium carbide phase dispersed in the nickel-tungsten composite matrix, wherein the titanium carbide phase is obtained by a substitution reaction between tungsten carbide and titanium.
[0008] In an optional embodiment, the average size of the titanium carbide phase is less than 1 μm;
[0009] And / or, the mass ratio of nickel to titanium in the nickel-tungsten powder is 1:(0.1-0.2);
[0010] And / or, the molar ratio of titanium, carbon and tungsten in the nickel-tungsten powder is 1:(0.9-1.1):(0.9-1.1).
[0011] In a second aspect, the present invention provides a method for preparing titanium carbide reinforced nickel-tungsten powder, comprising:
[0012] Vacuum melting, mixing the molten metal composed of nickel and titanium elements with tungsten carbide powder to obtain a composite molten metal;
[0013] Atomizing, atomizing the composite melt to obtain an atomized powder;
[0014] Heat treatment: heat treating the atomized powder to obtain the titanium carbide reinforced nickel-tungsten powder.
[0015] In an optional embodiment, the particle size of the tungsten carbide powder is less than 100 μm.
[0016] In an optional embodiment, the composite melt is obtained by adding tungsten carbide powder into the melt and mixing.
[0017] In an optional embodiment, the particle size of the atomized powder is ≤75 μm;
[0018] Preferably, the atomizing step comprises: using an inert gas to disperse and break the composite melt into droplets, and cooling the droplets to obtain atomized powder.
[0019] In an optional embodiment, the heat treatment temperature is 1000° C. to 1050° C., the time is 0.5 h to 1 h, and the vacuum degree is ≤100 Pa.
[0020] In a third aspect, the present invention provides a method for preparing a titanium carbide-reinforced nickel-tungsten alloy, comprising: using laser cladding to spray the titanium carbide-reinforced nickel-tungsten powder described in the aforementioned embodiment to obtain the titanium carbide-reinforced nickel-tungsten alloy.
[0021] In an optional embodiment, the cladding laser power is 1 kW to 2 kW;
[0022] and / or, the cladding speed is 1 mm / s to 5 mm / s;
[0023] And / or, the powder feeding rate is 60 g / min to 120 g / min.
[0024] In a fourth aspect, the present invention provides a titanium carbide reinforced nickel-tungsten alloy prepared by the method described in the aforementioned embodiment.
[0025] The present invention has the following beneficial effects:
[0026] In the present invention, the titanium carbide dispersed in the nickel-tungsten powder is obtained by a substitution reaction between tungsten carbide and titanium. During the substitution reaction, the titanium element combines with the carbon element to form a smaller and dispersed titanium carbide. The titanium carbide and the nickel-tungsten substrate are metallurgically combined to finally obtain titanium carbide dispersion-strengthened nickel-tungsten powder. Titanium carbide dispersion-strengthened nickel-tungsten alloy can be prepared by laser cladding method using the dispersion-strengthened powder. The titanium carbide dispersion-strengthened nickel-tungsten powder provided by the present invention has lower requirements on the particle size of the raw materials when it is prepared, and the nickel-tungsten powder has fewer defects. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0028] Figure 1 The flowchart of the method for preparing the titanium carbide reinforced nickel-tungsten powder of the present invention;
[0029] Figure 2 The microstructure of the titanium carbide dispersion strengthened nickel-tungsten powder prepared in Example 1;
[0030] Figure 3 The microstructure diagram of the titanium carbide dispersion strengthened nickel-tungsten alloy prepared in Example 1;
[0031] Figure 4 This is the microstructure diagram of the titanium carbide dispersion strengthened nickel tungsten powder prepared in Comparative Example 1. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0033] An embodiment of the present invention provides a titanium carbide reinforced nickel-tungsten powder, comprising a nickel-tungsten composite matrix and a titanium carbide phase dispersed in the nickel-tungsten composite matrix, wherein the titanium carbide phase is obtained by a substitution reaction between tungsten carbide and titanium.
[0034] In an embodiment of the present invention, titanium carbide dispersed in nickel-tungsten powder is obtained by substitution reaction between tungsten carbide and titanium. During the substitution reaction, titanium element combines with carbon element to form titanium carbide with smaller size and dispersed distribution. Titanium carbide and nickel-tungsten substrate are metallurgically combined to finally obtain titanium carbide dispersion-strengthened nickel-tungsten powder. Titanium carbide dispersion-strengthened nickel-tungsten alloy can be prepared by laser cladding method using the dispersion-strengthened powder. The titanium carbide dispersion-strengthened nickel-tungsten powder provided by the present invention has lower requirements on raw material particle size during preparation, and the nickel-tungsten powder has fewer defects.
[0035] In an alternative embodiment, the average size of the titanium carbide phase is less than 1 μm.
[0036] In an optional embodiment, the mass ratio of nickel to titanium in the nickel-tungsten powder is 1:(0.1-0.2). If the titanium content is too little, the content of titanium carbide formed by heat treatment will be too little, and the wear resistance of the alloy will be poor. If the titanium content is too much, the nickel-tungsten powder after heat treatment will be more brittle and have poor toughness. The mass ratio of nickel to titanium is 1:(0.1-0.2) which can take into account both toughness and wear resistance.
[0037] In an optional embodiment, the molar ratio of titanium, carbon and tungsten in the nickel-tungsten powder is 1:(0.9-1.1):(0.9-1.1), at which time, titanium and tungsten carbide can undergo a replacement reaction according to a stoichiometric ratio to obtain titanium carbide, so that the nickel-tungsten powder has a lower content of tungsten carbide and titanium. If the proportion of titanium is too small, tungsten carbide phase will remain in the nickel-tungsten powder; if the proportion of titanium is too large, too much titanium element will remain in the nickel-tungsten powder, forming a nickel-titanium intermetallic compound, which reduces the toughness of the matrix.
[0038] The present invention also provides a method for preparing titanium carbide reinforced nickel-tungsten powder. Figure 1 As shown, including:
[0039] Vacuum melting, mixing the molten metal composed of nickel and titanium elements with tungsten carbide powder to obtain a composite molten metal;
[0040] Atomizing, atomizing the composite melt to obtain an atomized powder;
[0041] Heat treatment: heat treating the atomized powder to obtain the titanium carbide reinforced nickel-tungsten powder.
[0042] In the prior art, in order to obtain titanium carbide dispersion-strengthened nickel-tungsten powder and alloy, it is usually necessary to composite nickel-tungsten metal particles and titanium carbide particles into granules and then sinter them at high temperature. However, the size of titanium carbide particles in the powder obtained by this conventional process is limited by the size of the raw materials used and is often large, and the pores in the powder cannot be completely discharged. The existing titanium carbide composite nickel-tungsten powder and cladding alloy generally have many defects and weak titanium carbide dispersion.
[0043] In an embodiment of the present invention, driven by thermodynamic free energy, large tungsten carbide particles decompose, and the tungsten element enters the nickel matrix to form a new nickel-tungsten matrix; the titanium element combines with the carbon element to form small-sized and dispersed titanium carbide, and the titanium carbide and the nickel-tungsten substrate are metallurgically bonded to finally obtain titanium carbide dispersion-strengthened nickel-tungsten powder.
[0044] In an optional embodiment, the particle size of the tungsten carbide powder is less than 100 μm. If the particle size of the raw tungsten carbide powder is greater than 100 microns, during the heat treatment process, due to the limited element diffusion rate, the tungsten carbide particles are easily unevenly distributed or the reaction is insufficient, which is not conducive to improving the performance of the nickel tungsten powder.
[0045] In an optional embodiment, the composite melt is obtained by adding tungsten carbide powder to the melt and mixing. In order to improve the uniformity of the composite melt, in the present invention, the nickel block and the titanium block are first melted into a liquid state during vacuum smelting, and then the tungsten carbide powder is added thereto. If the tungsten carbide is placed in the smelting furnace first, due to the large weight of the tungsten carbide itself, the tungsten carbide cannot enter the nickel-titanium melt located above it, and thus a uniform composite melt cannot be obtained; if the nickel block, the titanium block and the tungsten carbide powder are placed in the smelting furnace at the same time, since the particle size of the tungsten carbide powder is smaller than that of other bulk materials, the tungsten carbide powder will flow to the bottom of the smelting furnace, and thus a uniform composite melt cannot be formed.
[0046] In an optional embodiment, the particle size of the atomized powder is ≤75 μm, which is conducive to the subsequent laser cladding to prepare a relatively dense alloy. If the particle size of the atomized powder is greater than 75 μm, large particles of powder are prone to insufficient melting during laser cladding, resulting in reduced density of the alloy and affecting the bonding strength of the alloy.
[0047] In an optional embodiment, the atomizing step includes: using an inert gas to disperse the composite melt, breaking it into droplets, and cooling the droplets to obtain atomized powder.
[0048] In an optional embodiment, the heat treatment temperature is 1000° C. to 1050° C., the time is 0.5 h to 1 h, and the vacuum degree is ≤100 Pa.
[0049] The embodiment of the present invention utilizes the principle that titanium and tungsten carbide can undergo a replacement reaction at 1000-1050°C to convert tungsten carbide into titanium carbide. If the vacuum heat treatment temperature is lower than 1000°C and the holding time is lower than 0.5 hours, it is not conducive to the decomposition of tungsten carbide, and the chemical reaction between titanium and tungsten carbide is insufficient; if the heat treatment temperature is higher than 1050°C and the holding time is higher than 1 hour, the powder particles are prone to adhesion, reducing the fluidity of the prepared nickel-tungsten powder. If the vacuum degree is greater than 100Pa, the oxygen content in the ambient atmosphere of the powder is relatively higher, and oxidation is likely to occur on the powder surface, affecting the oxygen content of the powder, and the cladding alloy is prone to internal oxidation or cracking.
[0050] An embodiment of the present invention further provides a method for preparing a titanium carbide-reinforced nickel-tungsten alloy, comprising: using laser cladding to spray the titanium carbide-reinforced nickel-tungsten powder described in the aforementioned embodiment to obtain the titanium carbide-reinforced nickel-tungsten alloy.
[0051] In an optional embodiment, the cladding laser power is 1 kW to 2 kW; if the laser power is too low, the alloy is not dense; if the laser power is too high, it is easy to cause excessive chemical elements in the cladding substrate to enter the alloy coating, causing hybridization of the alloy elements.
[0052] In an optional embodiment, the cladding speed is 1 mm / s to 5 mm / s; if the cladding speed is too low, too much laser heat will be transferred to the substrate, causing hybridization of alloy elements in the coating; if the cladding speed is too high, some cladding areas are prone to leaking.
[0053] In an optional embodiment, the powder feeding rate is 60 g / min to 120 g / min. If the powder feeding rate is too low, serious oxidation of the powder is likely to occur; if the powder feeding rate is too high, part of the powder is likely to be insufficiently melted, forming powder accumulation in the alloy, resulting in an increase in porosity defects in the coating.
[0054] An embodiment of the present invention further provides a titanium carbide reinforced nickel-tungsten alloy, which is prepared by the method described in the aforementioned embodiment.
[0055] The titanium carbide-reinforced nickel-tungsten alloy in the embodiment of the present invention has high density and the titanium carbide is dispersedly distributed.
[0056] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0057] Example 1
[0058] This embodiment provides a method for preparing a titanium carbide dispersion strengthened nickel-tungsten alloy, comprising the following steps:
[0059] Step 1: Put 1kg of nickel block and 0.1kg of titanium block into a vacuum melting furnace for melting, then add 0.4kg of tungsten carbide powder with a particle size of less than 100μm into the melt, mix evenly to obtain a composite melt, atomize the composite melt and sieve the atomized powder to obtain an atomized powder with a particle size of less than 75μm.
[0060] Step 2: Put the atomized powder into a vacuum heat treatment furnace, the heat treatment temperature is 1000°C, the heat treatment holding time is 0.5 hours, the vacuum pressure is 100Pa, and titanium carbide dispersion strengthened nickel tungsten powder is obtained after heat treatment.
[0061] Step 3: Laser cladding the titanium carbide dispersion-strengthened nickel-tungsten powder obtained in step 2 with a cladding laser power of 1 kW, a cladding speed of 5 mm / s, and a powder feeding rate of 60 g / min to obtain titanium carbide dispersion-strengthened nickel-tungsten alloy.
[0062] Example 2
[0063] This embodiment provides a method for preparing titanium carbide dispersion strengthened nickel-tungsten alloy, which is different from Embodiment 1 only in that: in step 1, the mass of the added titanium block is 0.2 kg, and the mass of the tungsten carbide powder is 0.8 kg.
[0064] Example 3
[0065] This embodiment provides a method for preparing titanium carbide dispersion strengthened nickel-tungsten alloy, which is different from Embodiment 1 only in that: in step 2, the heat treatment temperature is 1050° C., and the heat treatment holding time is 1 hour.
[0066] Example 4
[0067] This embodiment provides a method for preparing titanium carbide dispersion strengthened nickel-tungsten alloy, which differs from Embodiment 1 only in that: in step three, the cladding laser power is 2 kW, the cladding speed is 1 mm / s, and the powder feeding rate is 120 g / min.
[0068] Comparative Example 1
[0069] This comparative example provides a method for preparing a titanium carbide dispersion-strengthened nickel-tungsten alloy, which differs from Example 1 only in that in step 1, the particle size of the added tungsten carbide is 120 μm.
[0070] Comparative Example 2
[0071] This comparative example provides a method for preparing titanium carbide dispersion-strengthened nickel-tungsten alloy, which differs from Example 1 only in that in step 1, the mass of the added titanium block is 0.3 kg, and the mass of the tungsten carbide powder is 1.2 kg.
[0072] Comparative Example 3
[0073] This comparative example provides a method for preparing titanium carbide dispersion strengthened nickel-tungsten alloy, which differs from Example 1 only in that in step 2, the heat treatment temperature is 1080°C.
[0074] Comparative Example 4
[0075] This comparative example provides a method for preparing titanium carbide dispersion strengthened nickel-tungsten alloy, which differs from Example 1 only in that in step three, the laser cladding power is 2.5 kW.
[0076] Comparative Example 5
[0077] This comparative example provides a method for preparing titanium carbide dispersion-strengthened nickel-tungsten alloy, which differs from Example 1 only in that in step 1, the mass of the added titanium block is 0.1 kg, and the mass of the tungsten carbide powder is 0.6 kg.
[0078] Comparative Example 6
[0079] This comparative example provides a method for preparing titanium carbide dispersion strengthened nickel-tungsten alloy, which differs from Example 1 only in that in step 2, the heat treatment temperature is 950°C.
[0080] Comparative Example 7
[0081] This comparative example provides a method for preparing titanium carbide dispersion strengthened nickel-tungsten alloy, which differs from Example 1 only in that in step three, the laser cladding power is 0.5 kW.
[0082] Test Case
[0083] The powder microstructure or cladding alloy structure prepared in each embodiment and comparative example was detected, and the titanium particles and matrix density in the powder or alloy were observed in particular. The detection method was electron microscope image analysis (JY / T 010-1996). At the same time, the sphericity of the powder (reference standard: YS / T 1491-2021 Nickel-based high-temperature alloy powder sphericity determination method scanning electron microscope method) and the bonding strength between the alloy and the substrate (HB5476-1991 thermal spray coating bonding strength test method) were detected. The test results are shown in Table 1. Among them, the microstructure of the powder after heat treatment in Example 1 and the microstructure of the prepared alloy are as follows: Figure 2 and Figure 3 , Comparative Example 1 alloy structure see Figure 4 .
[0084] Table 1
[0085]
[0086]
[0087] As can be seen from Table 1, compared with the comparative example, the powder and alloy obtained by adopting the scheme of the embodiment of the present invention are both microstructures of titanium carbide dispersion-strengthened nickel-tungsten, titanium carbide and nickel-tungsten substrate are metallurgically bonded, and the coating alloy has no porosity defects. Further, according to Example 1 and Comparative Example 1, it can be seen that the use of larger-sized tungsten carbide powder raw materials is likely to cause incomplete decomposition of tungsten carbide in the cladding alloy, and there are defects in the powder and alloy structure, low powder sphericity, and low alloy density and strength; according to Example 1 and Comparative Example 2, it can be seen that if the content of titanium and tungsten carbide raw materials added is too high, it is easy to cause the brittleness of the cladding alloy to increase, resulting in cracking of the metal matrix, and there are defects in the powder and alloy structure, low powder sphericity, and low alloy density and strength; according to Example 1 and Comparative Example 3, it can be seen that if the heat treatment temperature is too high, it is easy to cause the powders to stick to each other, resulting in the powder losing good fluidity and being unable to carry out cladding normally, and there are defects in the powder and alloy structure, low powder sphericity, and low alloy density and strength. The density and strength of the alloy are low; it can be seen from Example 1 and Comparative Example 4 that if the laser power is too high, it is easy to cause obvious internal oxidation of the metal matrix and hybridization of the substrate elements, defects in the powder and alloy structure, low powder sphericity, low alloy density and strength; it can be seen from Example 1 and Comparative Example 5 that if too little titanium and tungsten carbide are added, the titanium carbide content is small, and the alloy strength is low; it can be seen from Example 1 and Comparative Example 6 that if the heat treatment temperature is too low, tungsten carbide is not completely converted into titanium carbide, and defects in the powder and alloy structure, low powder sphericity, low alloy density and strength; it can be seen from Example 1 and Comparative Example 7 that if the laser cladding power is too low, defects in the alloy structure, and low alloy density and strength.
[0088] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A titanium carbide reinforced nickel-tungsten powder, It is characterized in that The invention comprises a nickel-tungsten composite matrix and a titanium carbide phase dispersed in the nickel-tungsten composite matrix, wherein the titanium carbide phase is obtained by substitution reaction between tungsten carbide and titanium.
2. The titanium carbide reinforced nickel-tungsten powder according to claim 1, It is characterized in that The average size of the titanium carbide phase is less than 1 μm; And / or, the mass ratio of nickel to titanium in the nickel-tungsten powder is 1:(0.1-0.2); And / or, the molar ratio of titanium, carbon and tungsten in the nickel-tungsten powder is 1:(0.9-1.1):(0.9-1.1).
3. A method for preparing the titanium carbide reinforced nickel-tungsten powder according to claim 1 or 2, It is characterized in that include: Vacuum melting, mixing the molten metal composed of nickel and titanium elements with tungsten carbide powder to obtain a composite molten metal; Atomizing, atomizing the composite melt to obtain an atomized powder; Heat treatment: heat treating the atomized powder to obtain the titanium carbide reinforced nickel-tungsten powder.
4. The method for preparing the titanium carbide reinforced nickel-tungsten powder according to claim 3, It is characterized in that The particle size of the tungsten carbide powder is less than 100 μm.
5. The method for preparing the titanium carbide reinforced nickel-tungsten powder according to claim 3, It is characterized in that The composite melt is obtained by adding tungsten carbide powder into the melt and mixing them.
6. The method for preparing the titanium carbide reinforced nickel-tungsten powder according to claim 3, It is characterized in that The particle size of the atomized powder is ≤75 μm; Preferably, the atomizing step comprises: using an inert gas to disperse and break the composite melt into droplets, and cooling the droplets to obtain atomized powder.
7. The method for preparing the titanium carbide reinforced nickel-tungsten powder according to claim 3, It is characterized in that The heat treatment temperature is 1000℃~1050℃, the time is 0.5h~1h, and the vacuum degree is ≤100Pa.
8. A method for preparing a titanium carbide reinforced nickel-tungsten alloy, It is characterized in that include: Laser cladding is used to spray the titanium carbide reinforced nickel-tungsten powder according to claim 1 or 2 to obtain the titanium carbide reinforced nickel-tungsten alloy.
9. The method for preparing the titanium carbide reinforced nickel-tungsten alloy according to claim 8, It is characterized in that The cladding laser power is 1kW to 2kW; and / or, the cladding speed is 1 mm / s to 5 mm / s; And / or, the powder feeding rate is 60 g / min to 120 g / min.
10. A titanium carbide reinforced nickel-tungsten alloy, It is characterized in that Prepared by the method of claim 8 or 9.
Citation Information
Patent Citations
Metallurgical composition embodying hard metal carbides, and method of making
CA1078225A
Preparation method of in-situ self-generated titanium carbide particle-reinforced nickel-based gradient coating
CN102268672A
TiC particle reinforced high-strength high-wear-resistance tungsten-based composite material and preparation method thereof
CN115747550A
In-situ synthesize (TiW) C granule reinforced Fe base composition and its preparation metod
CN1537963A
Tic-particle-reinforced fe-based composite material and method for preparing same
WO2022102805A1
Cited By
Laser surface coating method for refractory metal
CN120989612A