Solar cell of perovskite thin film based on silane reconstructed surface and preparation method of solar cell
By introducing a silane self-assembled layer into perovskite solar cells to interact with the perovskite surface, passivating defects and forming a cross-linked hydrophobic network, the efficiency and stability problems of perovskite solar cells are solved, achieving high-efficiency photoelectric conversion and long-term stability.
Patent Information
- Application Number
- CN202411112990.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
The photoelectric conversion efficiency and light stability of existing perovskite solar cells still need to be further improved, especially since surface and interface defects affect device performance and stability.
The perovskite thin film structure is constructed from the bottom up, including a substrate, an anode, an anode modification layer, a perovskite thin film layer, a silane self-assembled layer, an electron transport layer, and a cathode modification layer. Organosilanes such as PFDTES or TMAPTMS interact with the perovskite surface to passivate defects and form a cross-linked hydrophobic network to improve stability.
It significantly improves the photoelectric conversion efficiency and light stability of perovskite solar cells. The encapsulated device maintains high efficiency under continuous illumination, showing a significant improvement compared to the untreated device.
Smart Images

Figure CN119012731A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of perovskite solar cells, and in particular relates to a solar cell based on a perovskite film with a silane-reconstructed surface and a preparation method thereof. Background Art
[0002] Over the past decade, the photoelectric conversion efficiency (PCE) of perovskite solar cells has increased significantly, from 3.8% to 26.7%. Existing research is committed to further improving the photoelectric conversion efficiency and enhancing the stability of devices through innovative strategies (such as component engineering, low-dimensionality, new charge transport materials, defect passivation, etc.) to promote its commercialization.
[0003] Structural defects in perovskite solar cells mainly exist at grain boundaries, surfaces and interfaces, which act as traps for photogenerated free carriers and impair device performance. In addition, they are the main channels for ion migration and often serve as starting points for moisture, oxygen intrusion and photodegradation. Therefore, surface or interface engineering is one of the effective strategies to improve device performance and stability. Surface defects can be removed by tape or laser, which can significantly improve device performance and stability. The formation of a two-dimensional perovskite thin layer on top of a three-dimensional perovskite film is also widely used to fill cation / anion vacancies and inhibit charge recombination to improve device performance and enhance its stability.
[0004] The invention patent application with publication number CN113471366A discloses a method for preparing a 2D / 3D perovskite solar cell based on cyclohexylmethylamine iodide salt, in which cyclohexylmethylamine reacts with the excess PbI2 on the surface of the three-dimensional perovskite layer to generate two-dimensional perovskite in situ, and finally forms a 2D / 3D composite perovskite film. Compared with three-dimensional perovskite solar cell devices, the carrier recombination of 2D / 3D perovskite solar cell devices is reduced, the defect state density is reduced, and the open circuit voltage is greatly improved. After optimization, an efficiency of 22.06% is achieved, and the hysteresis effect of the battery is reduced. Two-dimensional perovskite can block the ion migration between the three-dimensional perovskite layer and the hole transport layer, and the hysteresis effect of the device is significantly reduced. The stability of the 2D / 3D composite perovskite solar cell device has been significantly improved, and it can still maintain more than 80% of its initial efficiency after being placed in the air for 50 days.
[0005] The invention patent application with publication number CN114388698A discloses a method for preparing high-efficiency perovskite solar cells with the assistance of pre-protonated aminopyridine. The method of the present invention is not only convenient, simple to operate, low in cost, and effective, but also solves the interfacial proton transfer behavior induced by the Lewis base passivation of interface defects. Compared with the commonly used strong alkaline Lewis base molecule passivation defect, this method constructs a 3D / 2D heterojunction perovskite film in situ without damaging the original perovskite surface crystal structure. It not only passivates the interface defects and greatly improves the efficiency of the perovskite solar cell, but also utilizes the intrinsic hydrophobic properties of the low-dimensional perovskite crystal to improve the long-term stability of the perovskite solar cell.
[0006] However, the photoelectric conversion efficiency of the perovskite solar cells disclosed in the above patents still needs to be further improved. Therefore, there is an urgent need to design perovskite solar cells with higher photoelectric conversion efficiency and light stability. Summary of the invention
[0007] The present invention provides a solar cell based on a perovskite film with a silane-reconstructed surface, and the solar cell has high photoelectric conversion efficiency and light stability.
[0008] The present invention provides a solar cell based on a perovskite film with a silane reconstructed surface, comprising a substrate, an anode, an anode modification layer, a perovskite film layer, a silane self-assembly layer, an electron transport layer, a cathode modification layer and a cathode arranged in sequence from bottom to top;
[0009] The silane self-assembled layer is a self-assembled layer formed by organic silane, and the organic silane is 1H,1H,2H,2H-perfluorooctyltriethoxysilane (PFDTES) or 3-(trimethoxysilyl)propyl-N,N,N-trimethylammonium chloride (TMAPTMS).
[0010] The tail group of the organosilane provided by the present invention includes fluorine atoms or ammonium radicals, which interact with perovskite, can passivate the surface defects of perovskite, reduce the defects of perovskite film, and thus improve the performance and stability of perovskite. Moreover, compared with the existing fluorosilanes, the tail group of the PFDTES provided by the present invention has a higher content of fluorine atoms, which can better passivate the defects on the surface of perovskite, and the cross-linked organosilane has a strong hydrophobicity, which can further improve the stability of the device.
[0011] Preferably, the structural formula of the 1H,1H,2H,2H-perfluorooctyltriethoxysilane is:
[0012]
[0013] Preferably, the structural formula of the 3-(trimethoxysilyl)propyl-N,N,N-trimethylammonium chloride is:
[0014]
[0015] Preferably, the material of the perovskite film layer is Cs 0.03 (FA 0.97 MA 0.03 ) 0.97 Pb(I 0.97 Br 0.03 )3 or Cs 0.1 FA 0.90 Pb(I 0.6 Br 0.4 )3.
[0016] Preferably, the anode is ITO;
[0017] The anode modification layer is NiO x / Me-4PACz、NiO x / MeO-4PACz、NiO x / 2PACz、NiO x / Me-2PACz or NiO x / Br-2PACz, wherein x is 1-1.5, Me-4PACz is [4-(3,6-dimethyl-9H-carbazol-9-yl)butyl]phosphoric acid;
[0018] The electron transport layer is PC 61 BM or C 60 ;
[0019] The cathode modification layer is BCP;
[0020] The cathode is Ag.
[0021] On the other hand, the present invention also provides a method for preparing a solar cell based on a perovskite thin film with a silane-reconstructed surface, comprising:
[0022] Spin coating NiO on ITO x thin layer, then on NiO x The anode modification layer was obtained by spin coating Me-4PACz on the thin layer;
[0023] Spin coating a perovskite precursor solution on the anode modification layer, and after the spin coating is completed, perform a first annealing to obtain a perovskite film;
[0024] Spin coating the chlorobenzene solution of the organosilane on the perovskite film again, and performing a second annealing to obtain a perovskite film with a silane-reconstructed surface, that is, forming a self-assembled layer on the perovskite film;
[0025] Then deposit PC 61BM and BCP, followed by Ag deposition, yield a solar cell based on a perovskite film with a silane-reconstructed surface.
[0026] The present invention uses organosilane to treat the surface of perovskite, which, on the one hand, suppresses the defects on the surface of perovskite, improves the photoelectric conversion efficiency, and reduces the attenuation sites of the device. On the other hand, the cross-linked protective layer formed on the surface further improves the stability of the film and the device. The spin coating process is used when preparing the perovskite film in the embodiment of the present invention, and the process method is simple and efficient.
[0027] Preferably, in the solution for spin coating the organosilane, the concentration of the organosilane is 1-100 mg / mL.
[0028] Preferably, the concentration of the spin-coated perovskite solution is 1-2 M, and the solvent is a mixed solvent of DMF and DMSO.
[0029] Preferably, the annealing temperature of the first annealing is 80-100° C., and the annealing time is 5-30 min.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The present invention utilizes the interaction between the tail functional group of the organosilane and the perovskite to passivate the perovskite, reduce defects, and improve performance and stability. Meanwhile, the cross-linked hydrophobic network can further protect the perovskite and improve stability.
[0032] The perovskite solar cell prepared by the present invention has a high photoelectric conversion efficiency and excellent light stability. The stability of the packaged device prepared by the strategy of the present invention is significantly improved compared with the untreated device under 1 standard sunlight. For the wide bandgap system, the fluorescence spectrum of the perovskite film prepared by the present invention does not change under continuous light for 100 hours. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Voltage-current curves of the solar cell prepared in Example 1 of the present invention and the solar cell prepared by the traditional 2D / 3D low-dimensionalization strategy provided in Comparative Example 1, with a test area of 0.05979 cm 2 The test light intensity is AM 1.5G100mW / cm 2 ;
[0034] Figure 2 A stability comparison diagram of a solar cell prepared in Example 1 of the present invention and a solar cell prepared by a traditional 2D / 3D low-dimensionalization strategy provided in Comparative Example 1;
[0035] Figure 3Voltage-current curves of the solar cell prepared in Example 2 of the present invention and the solar cell prepared by the traditional 2D / 3D low-dimensionalization strategy provided in Comparative Example 1, with a test area of 0.05979 cm 2 The test light intensity is AM 1.5G100mW / cm 2 ;
[0036] Figure 4 This is a stability comparison chart of the solar cell prepared in Example 2 of the present invention and the solar cell prepared by the traditional 2D / 3D low-dimensionality strategy provided in Comparative Example 1. DETAILED DESCRIPTION
[0037] The present invention will be further described below in conjunction with the accompanying drawings and specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples that do not specify specific conditions are usually based on the normal conditions reported in the literature or the conditions recommended by the manufacturer.
[0038] Example 1
[0039] The transparent conductive glass plated with ITO (anode) was ultrasonically cleaned with a cleaning agent, deionized water, acetone, isopropanol and anhydrous ethanol in sequence for 15 minutes, dried, and then treated with ultraviolet ozone for 20 minutes.
[0040] NiO x The thin layer was prepared by spin coating Ni(NO3)2·6H2O (1M) dissolved in ethylene glycol and ethylenediamine on the cleaned ITO at 4000 rpm for 20 seconds and then baked on a hot plate at 315°C for 60 minutes. The substrate was then transferred to a nitrogen glove box.
[0041] Me-4PACz (0.5 mg / mL) was spin-coated onto NiO at a speed of 4000 rpm. x surface for 40 s and then annealed at 100 °C for 10 min.
[0042] After that, the perovskite Cs 0.03 (FA 0.97 MA 0.03 ) 0.97 Pb(I 0.97 Br 0.03)3, the precursor solution is precursor solution A: FAI (1.65M), MACl (0.5M), PbI2 (1.73M), precursor solution B: MABr (1.65M), PbBr2 (1.65M) and precursor solution C: CsI (1.65M), PbI2 (1.65M) mixed in a volume ratio of 100:3:3, and the solvent is DMF / DMSO (4:1v / v). The prepared precursor solution was filtered before use. The precursor solution (50μL) was spin coated at 1000rpm for 10 seconds and 5000rpm for 30 seconds. Chlorobenzene (CB, 150μL) was dropped onto the film surface at the 20th second of spin coating. The film was then annealed at 100°C for 30 minutes.
[0043] Then, organosilane was spin-coated on the perovskite surface, and a chlorobenzene solution of 1H,1H,2H,2H-perfluorooctyltriethoxysilane (PFDTES) (25 μL, 10 mg mL -1 ) was spin coated at 5000 rpm for 30 seconds and annealed at 100°C for 10 minutes.
[0044] Then PC was deposited at 3000 rpm and 2000 rpm respectively. 61 BM (20 mg mL -1 , chlorobenzene) and BCP (0.5 mg mL -1 , isopropanol). Finally, at 4×10 -4 Ag (100 nm) was deposited in a vacuum chamber with a high vacuum of 3.3 Å.
[0045] The JV measurements were performed in a nitrogen glove box using a solar simulator (SS-F5-3A, Enlitech) and AM 1.5G spectroscopy. The intensity was calibrated to 100 mW cm using a certified standard silicon solar cell (SRC-2020, Enlitech). -2 For stability testing, the packaged devices were kept in an atmosphere with a humidity of 50±5% and a temperature of 35±5°C, under a white light emitting diode (LED) with a light intensity of 100mW / cm 2 Under continuous irradiation, the device was monitored at the maximum output power point. The effective area of the prepared device is 0.092 cm 2 , the test mask area is 0.05979cm 2 .
[0046] Example 2
[0047] Different from Example 1, the organosilane provided in this example is 3-(trimethoxysilyl)propyl-N,N,N-trimethylammonium chloride (TMAPTMS).
[0048] Comparative Example 1
[0049] The traditional 2D / 3D strategy for preparing perovskite films and devices comes from the literature Advanced Functional Materials, 2023, 33, 2307949.DOI:10.1002 / adfm.202307949; Nature Communications 2018, 9, 3021.DOI:10.1038 / s41467-018-05454-4.
[0050] Performance Analysis:
[0051] Figure 1 Given a light intensity of 100mW / cm 2 The current-voltage curves of the unmodified device and the device modified with PFDTES according to the strategy of the present invention under AM1.5 simulated sunlight irradiation, from which the PCE is obtained to be 23.0%.
[0052] Figure 2 The packaged device is stored in an atmosphere with a humidity of 50±5% and a temperature of 35±5℃, and the light intensity of the white light emitting diode (LED) is 100mW / cm 2 Under continuous irradiation, the device was monitored at the maximum output power point. The stability of the device prepared by PFDTES modification in the strategy of the present invention is significantly improved compared with the untreated device.
[0053] Figure 3 Given a light intensity of 100mW / cm 2 Current-voltage curves of the unmodified device and the device modified with TMAPTMS according to the strategy of the present invention under AM1.5 simulated sunlight irradiation, from which the PCE is obtained to be 23.0%.
[0054] Figure 4 The packaged device is stored in an atmosphere with a humidity of 50±5% and a temperature of 35±5℃, and the light intensity of the white light emitting diode (LED) is 100mW / cm 2 Under continuous irradiation, the device was monitored at the maximum output power point. The stability of the device prepared by TMAPTMS modification in the strategy of the present invention is significantly improved compared with the untreated device.
Claims
1. A solar cell based on a perovskite thin film with a silane-reconstructed surface, characterized in that: It includes a substrate, an anode, an anode modification layer, a perovskite film layer, a silane self-assembly layer, an electron transport layer, a cathode modification layer and a cathode which are arranged in sequence from bottom to top; The silane self-assembled layer is a self-assembled layer formed by organic silane, and the organic silane is 1H,1H,2H,2H-perfluorooctyltriethoxysilane or 3-(trimethoxysilyl)propyl-N,N,N-trimethylammonium chloride.
2. The solar cell based on the perovskite thin film with silane reconstructed surface according to claim 1, characterized in that: The structural formula of the 1H,1H,2H,2H-perfluorooctyltriethoxysilane is:
3. The solar cell based on the perovskite thin film with silane reconstructed surface according to claim 1, characterized in that: The structural formula of the 3-(trimethoxysilyl)propyl-N,N,N-trimethylammonium chloride is:
4. The solar cell based on the perovskite thin film with silane reconstructed surface according to claim 1, characterized in that: The material of the perovskite film layer is Cs 0.03 (FA 0.97 MA 0.03 ) 0.97 Pb(I 0.97 Br 0.03 )3 or Cs 0.1 FA 0.90 Pb(I 0.6 Br 0.4 )3.
5. The solar cell based on the perovskite thin film with silane reconstructed surface according to claim 1, characterized in that: The anode is ITO; The anode modification layer is NiO x / Me-4PACz、NiO x / MeO-4PACz、NiO x / 2PACz、NiO x / Me-2PACz or NiO x / Br-2PACz, wherein x is 1-1.5, Me-4PACz is [4-(3,6-dimethyl-9H-carbazol-9-yl)butyl]phosphoric acid; The electron transport layer is PC 61 BM or C 60 ; The cathode modification layer is BCP; The cathode is Ag.
6. A method for preparing a solar cell based on a perovskite thin film with a silane-reconstructed surface according to any one of claims 1 to 5, characterized in that: include: Spin coating NiO on ITO x thin layer, then on NiO x The anode modification layer was obtained by spin coating Me-4PACz on the thin layer; Spin coating a perovskite precursor solution on the anode modification layer, and after the spin coating is completed, perform a first annealing to obtain a perovskite film; Spin coating the chlorobenzene solution of the organosilane on the perovskite film again, and performing a second annealing to obtain a perovskite film with a silane-reconstructed surface, that is, forming a self-assembled layer on the perovskite film; Then deposit PC 61 BM and BCP, followed by Ag deposition, yield a solar cell based on a perovskite film with a silane-reconstructed surface.
7. The method for preparing a solar cell based on a perovskite thin film with a silane-reconstructed surface according to claim 6, characterized in that: In the spin coating of the organosilane solution, the concentration of the organosilane is 1-100 mg / mL.
8. The method for preparing a solar cell based on a perovskite thin film with a silane-reconstructed surface according to claim 6, characterized in that: The concentration of the spin-coated perovskite solution is 1-2 M, and the solvent is a mixed solvent of DMF and DMSO.
9. The method for preparing a solar cell based on a perovskite thin film with a silane-reconstructed surface according to claim 6, characterized in that: The annealing temperature of the first annealing is 80-100° C., and the annealing time is 5-30 minutes.