Target material polishing method

Through ultrasonic polishing combined with abrasive ultrasonic impact and chemical corrosion, the coating problem caused by the high surface roughness of the target material is solved, and the effect of reducing costs and improving efficiency is achieved.

CN119077596APending Publication Date: 2024-12-06LEADING THIN FILM MATERIALS (JIANGSU) CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411196106.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the production of semiconductor chips, the high surface roughness of the target material leads to tip discharge, affecting the coating quality and production efficiency, and the existing polishing methods are costly and inefficient.

Method used

Using ultrasonic polishing method, combining abrasive ultrasonic impact and chemical corrosion, the polishing liquid and abrasives of specific formulas can gradually reduce the surface roughness of the target material, including the rough and fine polishing process, control the mesh number of abrasives and acid concentration, and reduce chemical corrosion. .

Benefits of technology

Effectively reduce the surface roughness of the target material, reduce the presputtering time of the coating, reduce costs, improve production efficiency, and eliminate chemical corrosion during the finishing process, reducing polishing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005016452100000091
    Figure BDA0005016452100000091
  • Figure BDA0005016452100000101
    Figure BDA0005016452100000101
  • Figure BDA0005016452100000111
    Figure BDA0005016452100000111
Patent Text Reader

Abstract

The invention relates to a target material polishing method, and belongs to the technical field of metal processing. According to the method, the target material is polished through the ultrasonic polishing method, the target material is roughly polished through abrasive ultrasonic impact and chemical corrosion at the same time, the polishing solution used for rough polishing is controlled to adopt a specific formula, the mesh number of the abrasive used for ultrasonic polishing is controlled to be within a specific range, and the surface roughness of the target material can be effectively reduced; the pre-sputtering time of semiconductor coating is shortened, the coating cost is reduced, the coating production efficiency is improved, chemical corrosion is not needed in the accurate grinding process, and the polishing cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal processing, and in particular to a target material polishing method. Background Art

[0002] The most critical step in the semiconductor chip production process is physical vapor deposition, and metal targets are one of the key consumables of physical vapor deposition. Targets made of pure aluminum, aluminum alloy, pure titanium, pure tantalum, and pure copper are used in large quantities. When the surface roughness of the target is large, its surface usually has high tips. When high voltage is passed during sputtering, it will cause tip discharge and damage the wafer. In addition, the surface roughness of the target directly affects the pre-sputtering time, and also affects production efficiency and production costs. Therefore, it is necessary to explore a polishing method to reduce the surface roughness of the target. Summary of the invention

[0003] Based on the defects of the prior art, the purpose of the present application is to provide a target material polishing method to better reduce the surface roughness of the target material.

[0004] To achieve the above object, the present application provides a target material polishing method, comprising the following steps:

[0005] The target material is coarsely polished and finely polished by ultrasonic polishing, and then cleaned and dried to obtain the target target material;

[0006] The polishing liquid used for rough polishing contains the following components in percentage by weight: acid concentration 1.5% to 40%, ferric chloride 0 to 4%, and water 60% to 98.5%;

[0007] The mesh number of the abrasive used in the ultrasonic polishing is in the range of 200-3000 meshes.

[0008] The present application uses an ultrasonic polishing method to polish the target material. By simultaneously using abrasive ultrasonic impact and chemical corrosion to rough-polish the target material, and controlling the polishing liquid used for rough polishing to use a specific formula and the mesh size of the abrasive used for ultrasonic polishing to be within a specific range, the surface roughness of the target material can be effectively reduced, the pre-sputtering time of semiconductor coating can be reduced, the coating cost can be reduced, and the coating production efficiency can be improved. In addition, chemical corrosion is no longer required in the fine grinding process, which reduces the polishing cost.

[0009] Preferably, the acid comprises at least one of HF, HNO3 and HCl;

[0010] The target material is made of at least one of aluminum, aluminum alloy, copper, copper alloy, titanium, titanium alloy, tantalum and tantalum alloy.

[0011] Preferably, the material of the target is aluminum, and the polishing liquid used for rough polishing contains the following components in weight percentage: HF 1.89%, water 98.11%, and the volume percentage of abrasive in the polishing liquid is 5% to 9%. Compared with using HNO3, H2SO4 and / or HCl as the acid in the polishing liquid used for rough polishing, using a specific content of HF as the acid in the polishing liquid used for rough polishing, the polishing effect of pure aluminum target is better and the surface roughness is lower.

[0012] Preferably, the material of the target material is aluminum alloy, and the polishing liquid used for rough polishing contains the following components in weight percentage: HF 0.39%, HNO3 2.41%, HCl 0.53%, water 96.67%, and the volume percentage of abrasive in the polishing liquid is 18% to 22%. Under the synergistic effect of specific contents of HF, HNO3 and HCl, the polishing effect of the aluminum alloy target material is better and the surface roughness is lower. Among them, the aluminum alloy is preferably at least one of 606 aluminum alloy and 2024 aluminum alloy.

[0013] Preferably, the material of the target is copper, and the polishing liquid used for rough polishing contains the following components in weight percentage: HCl 2.7% to 8%, ferric chloride 3.2% to 5%, water 88.5 to 93%, and the volume percentage of abrasive in the polishing liquid is 8% to 12%. Under the synergistic effect of a specific content of HCl and ferric chloride, the polishing effect of the pure copper target is better and the surface roughness is lower. Compared with HF, HNO3 and / or H2SO4 as the acid in the polishing liquid used for rough polishing, the polishing effect of the pure copper target is better and the surface roughness is lower when HCl is used as the acid in the polishing liquid used for rough polishing. Compared with adding ferric nitrate to the polishing liquid, adding ferric chloride can make the polishing effect of the pure copper target better and the surface roughness lower.

[0014] Preferably, the material of the target is titanium, and the polishing liquid used for rough polishing contains the following components in weight percentage: HF 3.28%, HNO3 32.16%, water 64.56%, and the volume percentage of abrasive in the polishing liquid is 23% to 27%. Under the synergistic effect of a specific content of HF and HNO3, the polishing effect of the pure titanium target is better and the surface roughness is lower.

[0015] Preferably, the material of the target is tantalum, and the polishing liquid used for rough polishing contains the following components in weight percentage: HF 10.93%, HNO3 26.78%, water 62.29%, and the volume percentage of abrasive in the polishing liquid is 38% to 42%. Under the synergistic effect of a specific content of HF and HNO3, the polishing effect of pure tantalum target is better and the surface roughness is lower.

[0016] Preferably, during the ultrasonic polishing process, the mesh size of the abrasive used is gradually increased, and each time the target surface is polished until there are no visual scratches. The mesh size of the abrasive used in ultrasonic polishing is gradually increased, which can better improve the polishing effect and make the surface roughness of the target lower.

[0017] Preferably, the mesh number of the abrasive used for the rough polishing is 200 mesh, and the mesh numbers of the abrasive used for the fine polishing are 400 mesh, 800 mesh, 1200 mesh, 1500 mesh and 2000 mesh, respectively. By using the abrasives of the above specific mesh numbers for rough and fine polishing, the polishing effect can be better improved, and the surface roughness of the target material can be lowered.

[0018] Preferably, the abrasive used for ultrasonic polishing includes at least one of aluminum oxide, boron carbide, silicon carbide and corundum.

[0019] Preferably, the abrasive used for the rough polishing is diamond, and the abrasive used for the fine polishing is boron carbide. By using the abrasives of the above specific materials for rough and fine polishing, the polishing effect can be better improved, and the surface roughness of the target material can be lowered.

[0020] Preferably, the rough polishing is performed at 40-50° C. Controlling the rough polishing to be performed at this temperature can, on the one hand, avoid volatilization of the polishing liquid and cause changes in component concentrations, and on the other hand, make the polishing liquid have better chemical activity and better corrosion effect, thereby achieving better polishing effect and lower surface roughness of the target material.

[0021] Preferably, the polishing liquid used for the fine polishing is water, and is carried out at 20-40° C., and the volume percentage of the abrasive in the polishing liquid is 18%-22%. In the fine polishing process, chemical corrosion and heating are not required, and the target material can obtain a better polishing effect, thereby reducing production costs.

[0022] Preferably, the ultrasonic polishing further satisfies: the ultrasonic frequency is 26 to 35 kHz, and the liquid level of the polishing liquid is 10 to 15 mm higher than the upper surface of the target material.

[0023] Compared with the prior art, the beneficial effects of the present application are as follows: the present application utilizes an ultrasonic polishing method to polish a target material, and by simultaneously utilizing abrasive ultrasonic impact and chemical corrosion to rough-polish the target material, and controlling the polishing liquid used for rough-polishing to use a specific formula and the mesh size of the abrasive used for ultrasonic polishing to be within a specific range, the surface roughness of the target material can be effectively reduced, the pre-sputtering time of semiconductor coating can be reduced, the coating cost can be reduced, and the coating production efficiency can be improved. In addition, chemical corrosion is no longer required during the fine grinding process, thereby reducing the polishing cost. DETAILED DESCRIPTION

[0024] In order to better illustrate the purpose, technical scheme and advantages of the present application, the present application will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present application in detail, rather than to limit the present application. All other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application. The experimental reagents and instruments involved in the implementation of the present application are all commonly used ordinary reagents and instruments unless otherwise specified.

[0025] Example 1

[0026] This embodiment provides a target material polishing method, comprising the following steps:

[0027] Place the pure copper target with a diameter of 524mm and a thickness of 25.4mm steadily on the polishing table to ensure that the target does not shake up and down;

[0028] Add 200 mesh corundum powder into the chamber of the electric ultrasonic polisher, then add polishing liquid and make the liquid level 12mm higher than the upper surface of the target material, the volume percentage of corundum powder in the polishing liquid is 10%, heat to 45°C, then set the ultrasonic frequency to 26KHz on the control panel, aim the tool head of the ultrasonic transducer working handle at the surface of the target material and move back and forth for rough polishing, then rinse with pure water, and proceed to the next step of polishing if there are no scratches visually, wherein the polishing liquid contains the following components in weight percentage: 5.61% HCl, 3.89% ferric chloride, and 90.50% water;

[0029] Then, fine polishing is performed with 400 mesh, 800 mesh, 1200 mesh, 1500 mesh and 2000 mesh boron carbide powder in sequence, and each fine polishing satisfies the following conditions: pure water is used as the polishing liquid, and the liquid level of the polishing liquid is 12 mm higher than the upper surface of the target material, the volume percentage of boron carbide powder in the polishing liquid is 20%, the ultrasonic frequency is 26 KHz, the tool head of the ultrasonic transducer working handle is aimed at the surface of the target material and moved back and forth, and after rinsing with pure water, no scratches are observed visually before proceeding to the next step of polishing or stopping polishing;

[0030] Turn off the ultrasonic wave and blow dry with dry nitrogen to obtain the target material.

[0031] Example 2

[0032] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the ultrasonic frequency during the rough polishing and fine polishing processes is 30 kHz.

[0033] Example 3

[0034] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the ultrasonic frequency during the rough polishing and fine polishing processes is 35 kHz.

[0035] Example 4

[0036] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the polishing liquid used for rough polishing contains the following components in percentage by weight: 7.71% HCl, 3.57% ferric chloride, and 88.72% water.

[0037] Example 5

[0038] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the polishing liquid used for rough polishing contains the following components in percentage by weight: 3.08% HCl, 4.28% ferric chloride, and 92.64% water.

[0039] Example 6

[0040] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the polishing liquid used for rough polishing contains the following components in percentage by weight: 5.61% HF, 3.89% ferric chloride, and 90.50% water.

[0041] Example 7

[0042] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the polishing liquid used for rough polishing contains the following components in percentage by weight: 5.61% HNO3, 3.89% ferric chloride, and 90.50% water.

[0043] Example 8

[0044] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the polishing liquid used for rough polishing contains the following components in percentage by weight: 5.61% HCl, 3.89% ferric nitrate, and 90.50% water.

[0045] Example 9

[0046] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the temperature of the rough polishing process is 30° C., that is, the rough polishing steps are as follows:

[0047] Add 200 mesh corundum powder into the chamber of an electric ultrasonic polisher, then add polishing liquid and make the liquid level 12 mm higher than the upper surface of the target material, the volume percentage of corundum powder in the polishing liquid is 10%, heat to 30°C, then set the ultrasonic frequency to 26KHz on the control panel, aim the tool head of the ultrasonic transducer working handle at the surface of the target material and move back and forth for rough polishing, then rinse with pure water, and proceed to the next step of polishing if there are no scratches visually, wherein the polishing liquid contains the following components in weight percentage: 5.61% HCl, 3.89% ferric chloride, and 90.50% water.

[0048] Example 10

[0049] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the temperature of the rough polishing process is 60° C., that is, the rough polishing steps are as follows:

[0050] Add 200 mesh corundum powder into the chamber of an electric ultrasonic polisher, then add polishing liquid and make the liquid level 12 mm higher than the upper surface of the target material, the volume percentage of corundum powder in the polishing liquid is 10%, heat to 60°C, then set the ultrasonic frequency to 26KHz on the control panel, aim the tool head of the ultrasonic transducer working handle at the surface of the target material and move back and forth for rough polishing, then rinse with pure water, and proceed to the next step of polishing if there are no scratches visually, wherein the polishing liquid contains the following components in weight percentage: 5.61% HCl, 3.89% ferric chloride, and 90.50% water.

[0051] Embodiment 11

[0052] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Example 1 in that the target material used is a pure tantalum target material with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: HF 10.93%, HNO3 26.78%, water 62.29%, and the volume percentage of corundum powder in the polishing liquid is 40%.

[0053] Example 12

[0054] This embodiment provides a target polishing method. The target polishing method of this embodiment is different from that of Embodiment 1 in that the target used is a pure tantalum target with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in percentage by weight: HF 37.71%, water 62.29%, and the volume percentage of corundum powder in the polishing liquid is 40%.

[0055] Embodiment 13

[0056] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Example 1 in that the target material used is a pure tantalum target material with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: HNO3 37.71%, water 62.29%, and the volume percentage of corundum powder in the polishing liquid is 40%.

[0057] Embodiment 14

[0058] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the target material used is a pure aluminum target material with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: HF 1.89%, water 98.11%, and the volume percentage of corundum powder in the polishing liquid is 7%.

[0059] Embodiment 15

[0060] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Example 1 in that the target material used is a pure aluminum target material with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: HNO3 1.89%, water 98.1%, and the volume percentage of corundum powder in the polishing liquid is 7%.

[0061] Example 16

[0062] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Example 1 in that the target material used is a pure aluminum target material with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: 1.89% HCl, 98.1% water, and the volume percentage of corundum powder in the polishing liquid is 7%.

[0063] Embodiment 17

[0064] The present embodiment provides a target material polishing method. The target material polishing method of the present embodiment is different from that of Embodiment 1 in that the target material used is a 606 aluminum alloy target material with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: HF 0.39%, HNO3 2.41%, HCl 0.53%, water 96.67%, and the volume percentage of corundum powder in the polishing liquid is 20%.

[0065] Embodiment 18

[0066] This embodiment provides a target polishing method. The target polishing method of this embodiment is different from that of Example 1 in that the target used is a 606 aluminum alloy target with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: HF 3.33%, water 96.67%, and the volume percentage of corundum powder in the polishing liquid is 20%.

[0067] Embodiment 19

[0068] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Example 1 in that the target material used is a 606 aluminum alloy target with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: HNO3 3.33%, water 96.67%, and the volume percentage of corundum powder in the polishing liquid is 20%.

[0069] Embodiment 20

[0070] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Example 1 in that the target material used is a 606 aluminum alloy target with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: 3.33% HCl, 96.67% water, and the volume percentage of corundum powder in the polishing liquid is 20%.

[0071] Embodiment 21

[0072] The present embodiment provides a target polishing method. The target polishing method of the present embodiment is different from that of Embodiment 1 in that the target used is a 606 aluminum alloy target with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: 3.33% HF and HNO3 in total, 96.67% water, wherein the weight ratio of HF to HNO3 is 0.39:2.41, and the volume percentage of corundum powder in the polishing liquid is 20%.

[0073] Embodiment 22

[0074] The present embodiment provides a target polishing method. The target polishing method of the present embodiment is different from that of Embodiment 1 in that the target used is a 606 aluminum alloy target with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: 3.33% HF and HCl in total, 96.67% water, wherein the weight ratio of HF to HCl is 0.39:0.53, and the volume percentage of corundum powder in the polishing liquid is 20%.

[0075] Embodiment 23

[0076] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Example 1 in that the target material used is a 606 aluminum alloy target with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: 3.33% HNO3 and HCl in total, 96.67% water, wherein the weight ratio of HNO3 to HCl is 2.41:0.53, and the volume percentage of corundum powder in the polishing liquid is 20%.

[0077] Embodiment 24

[0078] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Example 1 in that the target material used is a pure titanium target material with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: HF 3.28%, HNO3 32.16%, water 64.56%, and the volume percentage of corundum powder in the polishing liquid is 25%.

[0079] Embodiment 25

[0080] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the target material used is a pure titanium target material with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: HF 35.44%, water 64.56%, and the volume percentage of corundum powder in the polishing liquid is 25%.

[0081] Embodiment 26

[0082] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the target material used is a pure titanium target material with a diameter of 524 mm and a thickness of 25.4 mm, and the polishing liquid used in the rough polishing process contains the following components in weight percentage: HNO3 35.44%, water 64.56%, and the volume percentage of corundum powder in the polishing liquid is 25%.

[0083] Comparative Example 1

[0084] This comparative example provides a target material polishing method, comprising the following steps:

[0085] Place the pure copper target with a diameter of 524mm and a thickness of 25.4mm steadily on the polishing table to ensure that the target does not shake up and down;

[0086] Polish with 200 mesh, 400 mesh, 800 mesh, 1200 mesh, 1500 mesh and 2000 mesh emery sandpaper in turn. Polish each time until there are no scratches visible before proceeding to the next step or stopping polishing.

[0087] Comparative Example 2

[0088] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the polishing liquid used in the rough polishing process is pure water and is not heated.

[0089] Comparative Example 3

[0090] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that the polishing liquid used in the rough polishing process is pure water.

[0091] Comparative Example 4

[0092] This embodiment provides a target material polishing method. The target material polishing method of this embodiment is different from that of Embodiment 1 in that ultrasonic waves are not used during the rough polishing process, and no abrasive is added (ie, no corundum powder is added).

[0093] Comparative Example 5

[0094] This comparative example provides a target material polishing method, comprising the following steps:

[0095] Place the pure tantalum target with a diameter of 524 mm and a thickness of 25.4 mm steadily on the polishing table to ensure that the target does not shake up and down;

[0096] Polish with 200 mesh, 400 mesh, 800 mesh, 1200 mesh, 1500 mesh and 2000 mesh emery sandpaper in turn. Polish each time until there are no scratches visible before proceeding to the next step or stopping polishing.

[0097] The surface roughness of the target materials obtained in the above embodiments and comparative examples was tested according to GB / T 1031-2009 "Surface Roughness Parameters and Values ​​of Surface Structure Profile Method". The standard stipulates that the roughness can only be 14 orders of magnitude (see Table 1 of the standard). The test results are shown in Table A.

[0098] Table A

[0099]

[0100]

[0101]

[0102] It can be seen from the above data that the surface roughness of the target material obtained in each embodiment of the present application is below 0.8 μm. Comparative Examples 1 and 5 use mechanical polishing, and the surface roughness of the target material obtained is relatively high; the polishing liquid used in the rough polishing of Comparative Examples 2 and 3 is pure water, and the surface roughness of the target material obtained is relatively high; Comparative Example 4 only uses chemical polishing without ultrasonic polishing, and the surface roughness of the target material obtained is relatively high.

[0103] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.

Claims

1. A target polishing method, It is characterized in that The following steps are involved: The target material is coarsely polished and finely polished by ultrasonic polishing, and then cleaned and dried to obtain the target target material; The polishing liquid used for rough polishing contains the following components in percentage by weight: acid concentration 1.5% to 40%, ferric chloride 0 to 4%, and water 60% to 98.5%; The mesh number of the abrasive used in the ultrasonic polishing is in the range of 200-3000 meshes.

2. The target polishing method according to claim 1, It is characterized in that The acid includes HF, HNO 3 and HCl; The target material is made of at least one of aluminum, aluminum alloy, copper, copper alloy, titanium, titanium alloy, tantalum and tantalum alloy.

3. The target polishing method according to claim 2, It is characterized in that The material of the target material is aluminum, and the polishing liquid used for the rough polishing contains the following components in weight percentage: HF 1.89%, water 98.11%, and the volume percentage of the abrasive in the polishing liquid is 5% to 9%; Alternatively, the target material is aluminum alloy, and the polishing liquid used for rough polishing contains the following components in percentage by weight: HF 0.39%, HNO 3 2.41%, HCl 0.53%, water 96.67%, and the volume percentage of abrasive in the polishing liquid is 18% to 22%; Or, the material of the target material is copper, and the polishing liquid used for the rough polishing contains the following components in weight percentage: HCl 2.7% to 8%, ferric chloride 3.2% to 5%, water 88.5% to 93%, and the volume percentage of the abrasive in the polishing liquid is 8% to 12%; Alternatively, the target material is titanium, and the polishing liquid used for rough polishing contains the following components in percentage by weight: HF 3.28%, HNO 3 32.16%, water 64.56%, and the volume percentage of abrasive in the polishing liquid is 23% to 27%; Or, the material of the target is tantalum, and the polishing liquid used for rough polishing contains the following components in percentage by weight: HF 10.93%, HNO 3 26.78%, water 62.29%, and the volume percentage of abrasive in the polishing liquid is 38% to 42%.

4. The target polishing method according to claim 1, It is characterized in that During the ultrasonic polishing process, the mesh size of the abrasive used is gradually increased, and each time the target material is polished until there is no visible scratch on the surface.

5. The target polishing method according to claim 4, It is characterized in that The mesh number of the abrasive used for the rough polishing is 200 mesh, and the mesh numbers of the abrasive used for the fine polishing are 400 mesh, 800 mesh, 1200 mesh, 1500 mesh and 2000 mesh respectively.

6. The target polishing method according to claim 1, It is characterized in that The abrasive used in the ultrasonic polishing includes at least one of aluminum oxide, boron carbide, silicon carbide and corundum.

7. The target polishing method according to claim 6, It is characterized in that The abrasive used for the rough polishing is diamond; the abrasive used for the fine grinding is boron carbide.

8. The target polishing method according to claim 1, It is characterized in that The rough polishing is carried out at 40-50°C.

9. The target material polishing method according to claim 1, It is characterized in that The polishing liquid used for the fine polishing is water and is carried out at 20-40° C. The volume percentage of the abrasive in the polishing liquid is 18%-22%.

10. The target material polishing method according to claim 1, It is characterized in that The ultrasonic polishing also meets the following requirements: the ultrasonic frequency is 26 to 35 kHz, and the liquid level of the polishing liquid is 10 to 15 mm higher than the upper surface of the target material.

Citation Information

Patent Citations

  • Device and method for polishing sapphire substrate material by ultrasound assisted chemical machinery

    CN101716745A