Preparation method of regeneration agent for hydrogen peroxide prepared by anthraquinone method
A technology of hydrogen peroxide and regenerant, applied in chemical instruments and methods, peroxide/peroxyhydrate/peroxyacid/superoxide/ozone, chemical recovery, etc., can solve the difficult control of operating process conditions and other problems, to achieve the effects of excellent physical and chemical properties, lower production costs, good social and economic benefits
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2016-01-13
Smart Images
Figure 1 Figure 2
Abstract
Description
technical field
[0001] The invention relates to the production technology of hydrogen peroxide industrial regeneration agent, in particular to a preparation method of hydrogen peroxide regeneration agent prepared by anthraquinone method. technical background
[0002] Hydrogen peroxide, its aqueous solution is commonly known as hydrogen peroxide, is a strong oxidizing agent, which can be used in bleaching agents, coloring agents, raw materials for inorganic or organic peroxides, oxidizing agents, bactericides, disinfectants, preservatives, electroplating solutions, rocket power fuel etc. The industrial production method for preparing hydrogen peroxide is mainly the anthraquinone method. The process is to prepare a working solution with an alkyl anthraquinone and an organic solvent. Under the conditions of a pressure of 0.30MPa, a temperature of 328-338K, and the presence of a catalyst, hydrogen gas is introduced. Hydrogenate alkylanthraquinones to alkylhydroanthraquinones, a...
Examples
Embodiment 1
[0024] (1) Add 50g of dilute nitric acid aqueous solution with a concentration of 10% by volume to the alumina powder, mix well, and make into strips;
[0025] (2) After drying in the shade at room temperature, calcination at 600K for 3h to obtain a strip-shaped carrier;
[0026] (3) Immerse the strip-shaped carrier in 1L of 0.8mol / L sodium hydroxide solution for 1 minute, take it out, and dry it at 350K for 3h.
Embodiment 2
[0028] Alumina powder 800g
[0029] (1) Add 100g of dilute nitric acid aqueous solution with a concentration of 20% by volume to the alumina powder, mix well, and make into strips;
[0030] (2) After drying in the shade at room temperature, calcination at 700K for 3.5h to obtain a strip-shaped carrier;
[0031] (3) Immerse the strip-shaped carrier in 800ml of 2mol / L sodium hydroxide solution for 10 seconds, take it out, and dry it at 370K for 3.5h.
Embodiment 3
[0033] Alumina powder 900g
[0034] (1) After mixing the alumina powder and the saffron powder, add 80g of glacial acetic acid aqueous solution with a concentration of 40% by volume, mix well, and make into a strip;
[0035] (2) After drying in the shade at room temperature, calcination at 780K for 4h to obtain a strip-shaped carrier;
[0036] (3) Immerse the strip-shaped carrier in 600ml of 3mol / L sodium hydroxide solution for 2 minutes, take it out, and dry it at 380K for 4h.