A cyclic corrosion test method in a cavity

By adopting the cyclic corrosion test method in the cavity during the automobile design stage, combining static salt spray test and vibration simulation to simulate the environmental conditions during the automobile use process, the problem of the inability of the existing technology to effectively solve the corrosion of the door and side circumference is achieved. More accurate corrosion data acquisition and structural optimization are achieved, reducing the risk of rust.

CN114166735BActive Publication Date: 2024-11-08CHERY AUTOMOBILE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111498915.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-09
Publication Date
2024-11-08
Estimated Expiration
2041-12-09

AI Technical Summary

Technical Problem

The existing technology cannot effectively solve the corrosion problems that occur during the use of car doors and side enclosures, resulting in damage to product sales and corporate image, and it is impossible to detect and solve these problems in a timely manner during the design stage.

Method used

The circulating corrosion test method in the cavity is used, combined with static salt spray test and vibration mount, and the environmental conditions of the car during use are simulated and corrosion in the cavity are accelerated by spraying dust, salt spray, temperature and humidity changes and pressure difference. , provides more accurate corrosion data to optimize body structural design.

Benefits of technology

This method can more effectively reflect the corrosion conditions of the doors and side circumferences of the car during use, provide a theoretical basis to optimize the body structure, quickly discover the risk of rust, reduce the possibility of corrosion, and improve the corrosion resistance of product design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114166735B_ABST
    Figure CN114166735B_ABST
Patent Text Reader

Abstract

The invention provides a cyclic corrosion test method in a cavity, wherein samples with cavities such as a whole vehicle, a body-in-white or a system component with four doors and two covers are cleaned, sprayed with dust, sprayed with salt mist, and vibrated, and then humidity is alternating, and finally cleaned. The method combines a static salt spray test method with a vibration bench. Dust is sprayed before the test begins, and dust, salt mist, and changes in temperature and humidity are pressed into the cavity through vibration and cleaning, combined with the pressure difference between the inside and outside of the cavity, to accelerate corrosion in the cavity, and to find out whether the vehicle body structure design is reasonable. The test result provides a theoretical basis for vehicle body structure optimization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of automobiles, and in particular relates to a cyclic corrosion test method in a cavity. Background Art

[0002] The doors and side panels of the cars that were published on the Auto Quality website were rusted, and this was not an isolated case. This shows that effective corrosion tests were not conducted during the design phase of the car, and this problem was not discovered in time, resulting in corrosion of the doors and side panels during use after the product was launched. The discovery of the above problems not only affected product sales, but also the corporate image, causing losses to the company.

[0003] In the prior art, conventional static corrosion tests on body-in-white and doors are obviously unable to reflect the problem of rust penetration of doors and side panels, and thus cannot provide effective information for automobile designers to solve the above problem.

[0004] It is very necessary to provide product corrosion information effectively in order to solve the problem of door and side panel corrosion during the use of the car during the design stage. Summary of the invention

[0005] The purpose of the present invention is to provide a cyclic corrosion test method in a cavity, which is used for cyclic corrosion tests of whole vehicles, white bodies or four-door and two-lid system components. The method combines a static salt spray test method with a vibration bench. Dust is sprayed before the test begins, and dust, salt spray, temperature and humidity changes are pressed into the cavity through vibration and cleaning, combined with the pressure difference between the inside and outside of the cavity, to accelerate the corrosion in the cavity. Whether the vehicle body structure design is reasonable can be found out. The test results provide a theoretical basis for optimizing the vehicle body structure.

[0006] The specific technical solutions of the present invention are as follows:

[0007] A cyclic corrosion test method in a cavity comprises the following steps:

[0008] 1) Sample cleaning;

[0009] 2) Spraying dust;

[0010] 3) Spraying salt mist;

[0011] 4) Vibration;

[0012] 5) Humidity alternation;

[0013] 6) Clean the sample again.

[0014] The sample described in step 1) is a system component of a whole vehicle, a body in white, four doors or two covers; the above samples have cavities, and the cyclic corrosion test can better reflect the cavity corrosion situation and provide a reference for subsequent improvements.

[0015] Furthermore, for the body-in-white as the sample, it is sealed before cleaning. The sealing scheme uses tooling parts for sealing. If the tooling parts do not meet the requirements for loading, the process holes are sealed with sealing materials. The sealing materials cannot accelerate the corrosion of the contact surface. After the sample is sealed, a sealing test is required.

[0016] Step 1) cleaning the sample is specifically as follows: at room temperature, the sample is cleaned with water, the surface of the sample is cleaned and then dried or wiped clean for later use; preferably, grade tertiary water is used for cleaning;

[0017] In step 1), the sample cleaning is to simulate car washing. During the use of the car, the vehicle will be exposed to rainwater and car washing water. The water will flow into the cavity of the sample (doors, body and other parts with cavities) along the gaps of the mounting parts and go down along the inner wall of the cavity. Part of the water will flow out through the drainage holes, and part of the water will accumulate at the overlap of the two plates where the water flow is not smooth. This place is in a humid environment for a long time, and the temperature and humidity change. The water film at the accumulation will go through a cycle of thick to thin and then thick again, which accelerates the corrosion of the contact surface of the water film.

[0018] The dust spraying in step 2) refers to taking the salt-ash mixture and spraying it evenly on the test surface to make the surface of the sample wet. The salt-ash mixture on the surface of the sample will flow into the gap of the lap joint along with the water film formed in the subsequent salt spray stage and the temperature and humidity stage, and finally enter the cavity. When encountering the temperature and humidity change test, it will accelerate the electrochemical corrosion in the cavity.

[0019] The salt-ash mixture refers to a salt-ash mixture of 10g / L±0.2g / L; the specific preparation method of the salt-ash mixture is: prepare 50g / L±5g / L sodium chloride solution with water, take dust and put it into the above sodium chloride solution to mix well, and prepare a salt-ash mixture with a dust concentration of 10g / L±0.2g / L; the dust used meets: ISO 12103-1 A2 FINE TEST DUST; the water used is grade 3 water;

[0020] In step 2), the spraying amount is 0.5±0.05L per square meter;

[0021] Step 2) After spraying the dust, let it stand for 30min±5min for use.

[0022] In step 3), the salt spray is 50g / L±5g / L sodium chloride solution as the electrolyte, and the spraying is carried out continuously for 60±5min at 35℃±2℃; wherein, after 20±5min of the salt spraying, the sample cavity is negatively pressurized for 40±5min, and the salt spray enters the cavity. The precipitation amount of the salt spray is controlled at 2-5ml / 80cm 2.h, pH of salt spray recovery liquid is 6.5-7.2; vacuum pump is used for negative pressure extraction, preferably Fujiwara 1550D, with appropriate pressure, which is conducive to salt spray entering the cavity and better simulating corrosion test.

[0023] Step 3) After the test, let it stand for 10±2 minutes for later use.

[0024] Step 3) The specific method is as follows: place the sample treated in step 2) in a multifunctional corrosion test chamber, use a spraying method combining a rocker-arm nozzle and a fixed nozzle to achieve a certain amount of corrosion intensity and corrosion uniformity, and examine the corrosion resistance of the sample; the salt spray is 50g / L±5g / L sodium chloride solution, and the spraying is continuous for 60min±5min. Among them, after 20±5min of salt spraying, the sample cavity is negatively pressurized for 40±5min; the precipitation amount of salt spray is controlled at 2-5ml / 80cm 2 .h, pH of salt spray recovery liquid 6.5-7.2;

[0025] Step 3) During the salt spraying stage, the sample is stationary and the spraying flow rate can meet the precipitation requirement.

[0026] The vibration described in step 4) is controlled at 120min±10min to simulate the vibration test of the short-term driving process of the vehicle during daily use. The vibration program can be selected according to the actual situation, and the vibration is turned on after installation and debugging. The adjacent parts of the sample will produce relative movement under vibration, and small cracks or gaps will appear in the welding and overlap joints. During the entire cycle test, the corrosive medium will enter the small cracks and gaps, causing electrochemical corrosion. Step 4) The vibration is carried out using the MTS four-pillar road simulation test machine or the side door system durability test bench. The system components with four doors or two covers use the side door system durability test bench, the sample is a whole vehicle using the MTS four-pillar road simulation test, and the sample is a white body and needs to be equipped with a whole vehicle for the MTS four-pillar road simulation test.

[0027] Step 5) Humidity alternation process: the test sample is moved to the temperature and humidity alternation box. During the entire humidity alternation process, the temperature remains unchanged and only the humidity changes. The humidity alternation is carried out in sequence according to the following procedures: 15 minutes, the temperature and humidity rise to 50℃±2℃ / (95±5)%RH—50℃±2℃ / (95±5)%RH, store for 2 hours—50℃±2℃ / (95±5)%RH, draw negative pressure in the cavity for 1 hour—50℃±2℃ / (95±5)%RH, store for 6 hours and 20 minutes—70±5min, the humidity drops to 50℃±2℃ / (60±5)%RH—15±2min, the humidity rises to 50℃±2℃ / (85±5)%RH—50℃±2℃ / 80-90%RH, store for 10h±10min

[0028] Through the above humidity alternation process, the wet-dry-wet process in the actual driving process is simulated, which better simulates the environmental changes of the car during driving, reflects the cavity corrosion factors of the actual car, and makes the corrosion test results more accurate.

[0029] Step 6) is to clean the vehicle again. The specific cleaning method is the same as step 1); step 6) is to simulate the process of cleaning the vehicle after using it for a period of time, to clean the dust and salt remaining on the surface of the sample, so as to facilitate the evaluation of the subsequent test results. This is the cleaning after the test, and the cleaning is convenient for the changes of the sample before and after the test.

[0030] After the test, the corrosion on the sample surface and in the cavity needs to be evaluated and recorded for qualitative analysis or evaluation of corrosion depth.

[0031] The inventor found that although the existing technology conducts static corrosion tests, corrosion still occurs in the actual use of the car. After research and exploration, the inventor found that due to the existence of the car cavity, the entire car is in a vibrating state during the actual use of the car. Therefore, the present invention simulates the vibration of the car driving by vibration to bring external corrosive media such as dust, rain, condensation, cleaning fluid, etc. into the cavity, and then aggravates the corrosion in the cavity through the changes in temperature and humidity during the day and night.

[0032] In the product design stage of the present invention, in order to avoid or reduce the risk of corrosion in the cavity, the present invention moves dust and vibration into the test room, combines the salt spray test and temperature and humidity changes, and presses the corrosive medium in the laboratory into the cavity through the pressure difference between the inside and outside of the cavity to accelerate the corrosion in the cavity. The method of the present invention can better reflect the actual use situation and provide more effective corrosion data for the product design stage.

[0033] Compared with the prior art, in order to be closer to the actual working conditions, the present invention combines vibration, dust, salt spray and temperature and humidity alternation procedures during the test process, and accelerates the corrosion in the cavity by generating a pressure difference between the inside and the outside, which can better simulate the corrosion perforation phenomenon that may exist in the actual application of automotive parts or components. The advantage of this test method is that it can quickly discover the corrosion risk in the cavity, and prevent or improve the occurrence of corrosion in the cavity through design optimization. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The following are photos of cavity corrosion during actual use of aftermarket vehicles as reported on the Auto Quality website (the circled position is the corrosion position);

[0035] Figure 2 This is a photo of the cavity corrosion of sample 1 after the simulation experiment of the present invention (the circled position is the corrosion position);

[0036] Figure 3This is a photo of the cavity corrosion of sample 2 after the simulation experiment of the present invention (the circled position is the corrosion position);

[0037] Figure 4 It is a schematic diagram of the process of the method of the present invention. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0040] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0041] Example 1 (Car door cyclic corrosion test case)

[0042] A cyclic corrosion test method in a cavity comprises the following steps:

[0043] 1) Sample cleaning: Clean with grade 3 water at room temperature, then dry or wipe clean, inspect and record whether the paint coating on the outer surface of the door is intact. The paint coating inspection and recording time should be completed within 30 minutes, and then proceed to step 2);

[0044] 2) Spraying dust: Use grade 3 water to prepare 50g / L sodium chloride solution, take dust and place it in the above sodium chloride solution to mix well, and prepare a salt-ash mixture with a dust concentration of 10g / L; the dust used meets: ISO 12103-1 A2 FINE TESTDUST; Take a certain amount of salt-ash mixture and spray it evenly on the surface of the door to make the door surface wet. This step does not require vibration. The salt-ash mixture on the surface of the sample will flow into the gap of the door lap part along with the water film formed in the salt spray stage and the temperature and humidity stage, and finally enter the cavity; if it encounters a temperature and humidity change test, it will accelerate the electrochemical corrosion in the cavity; the spraying amount is 0.5L per square meter, and it needs to stand for 30 minutes after spraying the dust before proceeding to step 3);

[0045] 3) Spraying salt mist: Using 50g / L sodium chloride solution as the electrolyte, place the door treated in step 2) in the corrosion test chamber. The temperature during the salt mist spraying stage is 35°C. 25 minutes after the salt mist spraying, the sample is subjected to negative pressure for 45 minutes (using Fujiwara 1550D). During the negative pressure pumping process, salt mist spraying is carried out simultaneously. The precipitation amount of salt mist is controlled at 3.0-4.0ml / 80cm 2 .h, the pH of the salt spray recovery liquid is 6.5-7.2, the sample is in a static state during the spraying process, and after the test, it is left to stand for 10 minutes before proceeding to step 4).

[0046] 4) Vibration durability: After the test in step 3), the vehicle door is transferred to the vehicle door durability test bench. After installation and commissioning, a 2-hour durability test is started. Adjacent parts of the specimen will produce relative movement under vibration, and small cracks or gaps will appear at welding and overlap joints. During the entire cycle test process, the corrosive medium will enter the small cracks and gaps, causing electrochemical corrosion.

[0047] 5) Temperature and humidity alternation process: Move the door after the test in step 4) to the temperature and humidity alternation box, and the temperature and humidity alternation procedure is: 15 minutes, temperature and humidity rise to 50℃ / 95%RH-50℃ / 95%RH storage for 120 minutes-50℃ / 95%RH negative pressure extraction for 60 minutes-50℃ / 95%RH storage for 380 minutes-50℃ condition humidity drops to 60%RH for 70 minutes-50℃ condition humidity rises to 85%RH for 15 minutes-50℃ / 85%RH storage for 600 minutes. Through the alternating changes of temperature and humidity, the surface of the sample is in a "wet-dry-wet" alternation process.

[0048] Step 6) Clean again: clean the dust and salt remaining on the door surface to facilitate subsequent tests and evaluation of test results.

[0049] Step 1) to step 6) is a cycle, and after a total of 6 cycles of testing, the corrosion on the door surface and in the cavity needs to be evaluated and recorded, and the corrosion depth needs to be evaluated qualitatively or evaluated;

[0050] After the test, the corrosion evaluation of the door surface and cavity should be carried out and recorded. Figure 2 , Figure 3 ) It can be concluded that the rust location of this test method is different from the after-sales failure location ( Figure 1 ). Figure 1 It can be seen that the after-sales failure position is under the car door. Figure 1 The circled position is the corrosion position after the vehicle has been used for a period of time. Figure 2 , Figure 3 The circled position is the rusted position after the experiment. Figure 1The positions are consistent. The method of the present invention can effectively reflect the actual corrosion situation. The method designed according to the present invention can accelerate the corrosion in the cavity to find out whether the design of the vehicle body structure is reasonable, providing a theoretical basis for the optimization of the vehicle body structure.

Claims

1. A cyclic corrosion test method in a cavity, characterized in that: The method comprises the following steps: 1) Sample cleaning; 2) Spraying dust; 3) Spraying salt mist; 4) Vibration; 5) Humidity alternation; 6) Clean the sample again; The dust spraying in step 2) refers to spraying the salt-ash mixture evenly on the test surface; the specific preparation method of the salt-ash mixture is: prepare 50g / L±5g / L sodium chloride solution with water, take the dust and mix it in the sodium chloride solution to prepare a salt-ash mixture with a dust concentration of 10g / L±0.2g / L; Step 5) Humidity alternation is carried out in sequence according to the following procedures: Humidity alternation is carried out in sequence according to the following procedures: 15 minutes, temperature and humidity rise to 50℃±2℃ / (95±5)%RH—50℃±2℃ / (95±5)%RH, store for 2 hours—50℃±2℃ / (95±5)%RH, draw negative pressure in the cavity for 1 hour—50℃±2℃ / (95±5)%RH, store for 6 hours and 20 minutes—70±5min, humidity drops to 50℃±2℃ / (60±5)%RH—15±2min, humidity rises to 50℃±2℃ / (85±5)%RH—50℃±2℃ / 80-90%RH, store for 10h±10min.

2. The method according to claim 1, characterized in that The sample in step 1) is a system component of a whole vehicle, a body in white, four doors or two lids.

3. The method according to claim 1, characterized in that In step 2), the spraying amount is 0.5±0.05L per square meter.

4. The method according to claim 1, characterized in that In step 3), the salt mist sprayed is 50g / L±5g / L sodium chloride solution as the electrolyte, and the spraying is carried out continuously for 60±5min at 35℃±2℃; 20±5min after the salt mist spraying, the negative pressure is drawn to the sample cavity for 40±5min.

5. The method according to claim 1 or 4, characterized in that: In step 3), the precipitation amount of salt spray is controlled at 2-5ml / 80cm 2 .h, pH of salt spray recovery liquid is 6.5-7.

2.

6. The method according to claim 1, characterized in that The vibration in step 4) is performed for 120 min±10 min.