Formulation for high porosity chemical mechanical polishing pad with high hardness and CMP pad made therefrom
By using a two-component reaction mixture of liquid aromatic isocyanate and polyol components, a polyurethane foam polishing pad with specific hardness and density is formed, which solves the defect rate problem of CMP polishing pads when improving removal rate and hardness, and achieves a more flexible performance window and uniformity.
Patent Information
- Application Number
- CN202210058958.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-01-21
- Filing Date
- 2022-01-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-01-18
AI Technical Summary
Existing CMP polishing pads tend to increase the defect rate when improving removal rate and hardness, making it difficult to balance performance trade-offs.
A two-component reaction mixture of liquid aromatic isocyanate and liquid polyol is used to form a polyurethane foam polishing pad with specific hardness and density by controlling the gelation time and porosity. Combined with a suitable polishing layer and bottom side pad, the polishing performance is optimized.
It achieves improved removal rate and hardness at low defect rates, provides a more flexible performance window, is suitable for polishing magnetic, optical and semiconductor substrates, reduces density and improves the uniformity and reproducibility of polished layers.
Smart Images

Figure BDA0003474596330000171
Abstract
Description
[0001] The present invention relates to a two-component polyurethane composition for preparing a chemical mechanical planarization polishing (CMP polishing) pad having a Shore DO hardness (15 seconds) of 40 or more and a specific gravity (SG) of 0.5 or less, a CMP polishing pad prepared therefrom, and a method for preparing the same. More specifically, the present invention relates to a CMP polishing pad comprising a polyurethane foam reaction product of a two-component reaction mixture of a liquid aromatic diisocyanate component and a liquid polyol component (comprising a short-chain diol and a liquid aromatic diamine curing agent), wherein the liquid polyol component contains, for example, water in an amount of 1000 to 8500 ppm based on the total weight of the two-component reaction mixture.
[0002] In the CMP process, a polishing pad is combined with a polishing solution (such as an abrasive-containing polishing slurry and / or an abrasive-free reactive liquid) to remove excess material in a manner that planarizes or maintains the flatness of a semiconductor, optical, or magnetic substrate. There is a continuing need for CMP polishing pads that have increased layer uniformity or planarization performance combined with acceptable removal rates. However, there is still a performance tradeoff in the industry between removal rate or hardness and defectivity, where greater removal rate or hardness results in more defects.
[0003] Itoyama et al., U.S. Patent Publication No. US2014 / 0038503A1, discloses a method for making molded CMP polishing pads of polyurethane-urea foam having a foaming capacity of 0.30 to 0.60 g / cm 3 The Itoyama pad has a density of 5 to 35 degrees and a D-type hardness of 5 to 35 degrees (JISK 6253-1997 / ISO 7619). The formulation for the CMP polishing pad comprises a mixture of an isocyanate compound, a polyisocyanate compound, a polyamine compound and an aqueous dispersion mixture (comprising water, a foam stabilizer, a reaction catalyst and a non-reactive gas). The composition further comprises a polyol, which is disclosed as having a number average molecular weight of 500 to 5000. The Itoyama pad includes pores produced by the reaction of water and isocyanate; however, the disclosed pad is soft because if the hardness is too high, scratches or defects will be formed on the polished substrate. See
[0076] .
[0004] The inventors of the present invention have sought to solve the problem of providing a more flexible formulation window for making chemical mechanical polishing layers or pads having improved hardness and removal rate properties without undesirably increasing defectivity. Summary of the invention
[0005] 1. According to the present invention, the organic solvent-free reaction mixture for forming a chemical mechanical polishing (CMP polishing) layer comprises: (i) a liquid aromatic isocyanate component comprising one or more aromatic diisocyanates or linear aromatic isocyanate-terminated urethane prepolymers, preferably linear methylene diphenyl diisocyanate (MDI) prepolymers, having an unreacted isocyanate (NCO) concentration of 18 to 40 wt.%, or preferably 18 to 34 wt.%, based on the total solid weight of the liquid aromatic isocyanate component, and (i i) a liquid polyol component comprising a) one or more polymer polyols such as polytetramethylene glycol (PTMEG), polypropylene glycol (PPG), hexafunctional polyols, or mixtures thereof, b) based on the total weight of the liquid polyol component, 15 to 36 wt.% of one or more small chain difunctional polyols having 2 to 6 carbon atoms, such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 2-methyl-1,3-propanediol, 1,4-butylene glycol, neopentyl glycol. %, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, tripropylene glycol and mixtures thereof, or preferably ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol and / or triethylene glycol, and c) 0 to 25 wt.% of a liquid aromatic diamine, based on the total weight of the liquid polyol component, the liquid aromatic diamine being liquid at standard pressure and 40° C., and d) sufficient to reduce the density of a CMP polishing pad made from the two-component reaction mixture to 0.2 to 0.50 g / mL or preferably % or preferably 0.4 to 2.5 wt. % of CO2-amine adducts, based on the total weight of the two-component reaction mixture, wherein the reaction mixture comprises 60 to 75 wt. % or preferably greater than 63 to 75 wt. % of hard segment materials, based on the total weight of the reaction mixture. The two-component reaction mixture does not contain trace elements other than those formed by the water or CO2-amine adducts.
[0006] 2. According to the present invention, the organic solvent-free reaction mixture for forming a chemical mechanical polishing (CMP polishing) layer as in item 1 above, wherein the reaction mixtures have a gel time of 15 seconds to 3 minutes or preferably 15 seconds to 2 minutes at 65°C.
[0007] 3. According to a separate aspect of the present invention, a chemical mechanical (CMP) polishing pad for polishing a substrate selected from at least one of a magnetic substrate, an optical substrate and a semiconductor substrate, the polishing pad comprising a polishing layer adapted to polish the substrate, the polishing layer comprising a polyurethane reaction product of a two-component reaction mixture free of an organic solvent, the two-component reaction mixture comprising: (i) a liquid aromatic isocyanate component comprising one or more aromatic diisocyanates or linear aromatic isocyanate-terminated urethane prepolymers, preferably linear methylene diphenyl diisocyanate (MDI) prepolymers, having 18 to 40 wt.%, or preferably 18 to 34 wt.%, of unreacted isocyanate (based on the total solid weight of the aromatic isocyanate component); NCO) concentration, and (ii) a liquid polyol component comprising a) one or more polymer polyols such as polytetramethylene glycol (PTMEG), polypropylene glycol (PPG), hexafunctional polyols, or mixtures thereof, b) 15 to 36 wt.% of one or more small chain difunctional polyols having 2 to 6 carbon atoms, such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, tripropylene glycol, and mixtures thereof, or preferably ethylene glycol, propylene glycol, tripropylene glycol, and mixtures thereof, based on the total weight of the liquid polyol component. % of a liquid aromatic diamine, which is liquid under ambient conditions, such as any one of dimethylthiotoluenediamine, toluenediamine, tert-butyltoluenediamine (such as 5-tert-butyl-2,4-toluenediamine or 3-tert-butyl-2,6-toluenediamine), chlorotoluenediamine and N,N'-dialkylaminodiphenylmethane and mixtures thereof, or preferably chlorotoluenediamine, dimethylthiotoluenediamine and mixtures thereof; diethyltoluenediamine (DETDA) and N,N'-dialkylaminodiphenylmethane, and d) sufficient to reduce the density of the CMP polishing pad to 0.2 to 0.50 g / cm3. %, or preferably 0.35 to 0.495 g / mL of water or CO2-amine adducts, such as CO2-alkanolamines, such as 1000 and 8500 ppm or preferably 1000 and 5000 ppm of water or 0.25 to 4.0 wt.% or preferably 0.4 to 2.5 wt.% of CO2-amine adducts, such as CO2-alkanolamines, based on the total weight of the two-component reaction mixture, wherein the reaction mixture comprises 60 to 75 wt.%, or preferably greater than 63 to 75 wt.% of hard segment materials based on the total weight of the reaction mixture, wherein the CMP polishing layer has a Shore DO (15 seconds) hardness of 40 to 80, or preferably at least 43, or 43 to 80, and has a Shore DO (15 seconds) hardness of 0.2 to 0.55 g / mL, or preferably 0.35 to 0.50 g / mL, or even more preferably 0.35 to 0.495 g / mL; preferably, further wherein the CMP polishing layer contains no trace elements other than those formed by the water or CO2-amine adduct. .
[0008] 4. A CMP polishing pad or reaction mixture according to the present invention as in any one of items 1, 2 or 3 above, wherein the stoichiometric ratio of the sum of the total moles of amine (NH2) groups and the total moles of hydroxyl (OH) groups in the reaction mixture to the total moles of unreacted isocyanate (NCO) groups in the reaction mixture for producing the CMP polishing layer is 0.85:1.0 to 1.15:1.0, or preferably 0.9:1.0 to 1.1:1.0.
[0009] 5. A CMP polishing pad according to the present invention as in any one of items 3 or 4 above, wherein the (i) liquid aromatic isocyanate component comprises one or more diisocyanates or isocyanate-terminated linear urethane prepolymer compounds selected from the group consisting of methylene diphenyl diisocyanate (MDI); toluene diisocyanate (TDI); naphthalene diisocyanate (NDI); p-phenylene diisocyanate (PPDI); or o-toluidine diisocyanate (TODI); a mixture thereof; any one of MDI, TDI, NDI, PPDA, TODI extended with one or more extender compounds having a molecular weight of 84 to 100 W; t.%, or preferably 90 to 100 wt.% of a linear isocyanate-terminated urethane prepolymer or a mixture thereof having a hard segment material content of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 2-methyl-1,3-propanediol, 1,4-butylene glycol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, tripropylene glycol and mixtures thereof, preferably a linear isocyanate-terminated urethane prepolymer of MDI (which is MDI or MDI dimer extended with one or more extender compounds).
[0010] 6. A CMP polishing pad according to the invention as in any one of items 3, 4 or 5 above, wherein the liquid aromatic diamine curing agent is liquid under ambient conditions and is selected from: dimethylthiotoluenediamine, a mixture of isomers 2,4-diamino-3,5-dimethylthiotoluene and 3,5-dimethylthio-2,4-toluenediamine; diethyltoluenediamine; tert-butyltoluenediamine, such as 5-tert-butyl-2,4-toluenediamine or 3-tert-butyl-2,6-toluenediamine; chlorotoluenediamine; and N,N'-dialkylaminodiphenylmethane and mixtures thereof, or preferably chlorotoluenediamine or dimethylthiotoluenediamine, a mixture of isomers 2,4-diamino-3,5-dimethylthiotoluene and 3,5-dimethylthio-2,4-toluenediamine, diethyltoluenediamine (DETDA) and N,N'-dialkylaminodiphenylmethane.
[0011] 7. A chemical mechanical polishing pad according to the present invention as in any one of items 1, 2, 3, 4, 5 or 6 above, which comprises the CMP polishing layer and further comprises a subpad or backing layer on the bottom side of the polishing layer, such as a polymer-impregnated nonwoven or polymer sheet, so that the polishing layer forms the top of the polishing pad.
[0012] 8. In yet another aspect, the present invention provides a method for making a chemical mechanical (CMP) polishing pad having a polishing layer adapted to polish a substrate, the method comprising providing a two-component reaction mixture as in any one of items 1, 2, 3, 4, 5 or 6 above, such as mixing the (i) liquid aromatic isocyanate component and the (ii) liquid polyol component in a static mixer or an impact mixer, and applying the reaction mixture as one component to an open mold surface (preferably having a positive topography forming a negative groove pattern in the top surface of the CMP polishing pad), curing the reaction mixture at ambient temperature to 130°C to form a molded polyurethane reaction product, for example, initially curing at ambient temperature to 130°C for a period of 1 to 30 minutes, or preferably 30 seconds to 5 minutes, removing the polyurethane reaction product from the mold, and then, finally curing at a temperature of 60°C to 130°C for a period of 1 minute to 16 hours, or preferably 5 minutes to 15 minutes.
[0013] 9. According to the method of the present invention as in item 8 above, the formation of the polishing pad further includes stacking a sub-pad layer such as a polymer-impregnated nonwoven, or a porous or non-porous polymer sheet onto the bottom side of the polishing layer so that the polishing layer forms the top surface of the polishing pad.
[0014] 10. The method according to the present invention as in any one of items 8 or 9 above, wherein the method forms the surface of the CMP polishing pad directly in the mold.
[0015] 11. A method according to the present invention as in any of items 8, 9 or 10 above, wherein applying the reaction mixture as a component includes overspraying the mold, followed by curing to form a polyurethane reaction product, removing the polyurethane reaction product from the mold, and then punching or cutting the periphery of the polyurethane reaction product to the desired diameter of the CMP polishing pad.
[0016] 12. On the other hand, the present invention provides a method for polishing a substrate, which comprises: providing a substrate selected from at least one of a magnetic substrate, an optical substrate and a semiconductor substrate; providing a chemical mechanical (CMP) polishing pad according to any one of items 1 to 7 above; generating dynamic contact between the polishing surface of the polishing layer of the CMP polishing pad and the substrate to polish the surface of the substrate; and adjusting the polishing surface of the polishing pad with an abrasive conditioner.
[0017] Unless otherwise indicated, temperature and pressure conditions are ambient temperature and standard pressure.All recited ranges are inclusive and combinable.
[0018] Unless otherwise indicated, any term containing brackets refers alternatively to the entire term as if no brackets were present and to the term without brackets, and to each alternative combination. Thus, the term "(poly)isocyanate" refers to an isocyanate, a polyisocyanate, or a mixture thereof.
[0019] All ranges are inclusive and combinable. For example, the term "50 cPs to 3000 cPs, or 100 cPs or more" would include each of 50 cPs to 100 cPs, 50 cPs to 3000 cPs, and 100 cPs to 3000 cPs.
[0020] For the purposes of the present invention, reaction mixtures are expressed in wt. %, unless specifically stated otherwise.
[0021] As used herein, the term "ASTM" refers to publications of ASTM International, West Conshohocken, PA.
[0022] As used herein, the term "average number of isocyanate groups" means the weighted average of the number of isocyanate groups in a mixture of aromatic isocyanate compounds. For example, a 50:50 wt.% mixture of MDI (2 NCO groups) and the isocyanurate of MDI (considered to have 3 NCO groups) has an average of 2.5 isocyanate groups.
[0023] As used herein, the term "gel time" means the result obtained by mixing a given reaction mixture at about 65°C, for example, in a VM-2500 vortex laboratory mixer (StateMix Ltd., Winnipeg, Canada) (set at 1000 rpm) for 30 s, setting the timer to zero and starting the timer, pouring the mixture into an aluminum cup, placing the cup on a gel timer (Gardco Hot Pot TM The reaction mixture was stirred at 20 RPM using a wire stirrer in a gel timer (Paul N. Gardner Company, Inc., Pompano Beach, FL) hot pan (set at 65°C) and the gel time was recorded when the wire stirrer stopped moving through the sample.
[0024] As used herein, the term "hard segment" of a polyurethane reaction product or raw material from any of a liquid polyol component and a liquid aromatic isocyanate component refers to a portion of a specified reaction mixture comprising any diol, glycol, diglycol, tri(glycol) having 6 or fewer carbon atoms, any diamine, triamine or polyamine, diisocyanate, triisocyanate, or a reaction product thereof. Thus, a "hard segment" does not include polyethers or polyglycols such as polyethylene glycol or polypropylene glycol, or polyoxyethylenes having three or more ether groups.
[0025] As used herein, the term "trace elements other than those formed by water or CO2-amine adducts" means trace elements selected from hollow core polymer materials such as polymer microspheres, liquid-filled hollow core polymer materials such as fluid-filled polymer microspheres, and fillers such as boron nitride. Pores formed in the CMP polishing layer by gases or foaming agents that simply form gases such as CO2-amine adducts are not considered trace elements.
[0026] As used herein, the term "polyisocyanate" means any isocyanate group-containing molecule containing two or more isocyanate groups.
[0027] As used herein, the term "polyisocyanate prepolymer" means any isocyanate group-containing molecule that is the reaction product of an excess of a diisocyanate or polyisocyanate and an active hydrogen-containing compound containing two or more active hydrogen groups, such as diamines, diols, triols and polyols.
[0028] As used herein, the term "polyurethane" refers to polymerization products derived from difunctional or polyfunctional isocyanates, such as polyether ureas, polyisocyanurates, polyurethanes, polyureas, polyurethane ureas, copolymers thereof, and mixtures thereof.
[0029] As used herein, the term "reaction mixture" includes any non-reactive additives, such as trace elements and any additives that reduce the hardness of the polyurethane reaction product in the CMP polishing pad according to ASTM D2240-15 (2015).
[0030] As used herein, the term "stoichiometry" of a reaction mixture refers to the ratio of molar equivalents of (free OH + free NH2 groups) to free NCO groups in the reaction mixture.
[0031] As used herein, the term "SG" or "specific gravity" refers to the weight / volume ratio of a rectangle cut from a polishing pad or layer according to the present invention.
[0032] As used herein, the term "Shore DO Hardness" is the 15-second hardness of a given CMP polishing pad as measured in accordance with ASTM D2240-15 (2015), "Standard Test Method for Rubber Property—Durometer Hardness." Hardness is measured on a Rex Hybrid hardness tester (Rex Gauge Company, Inc., Buffalo Grove, IL) equipped with an O probe. For each hardness measurement, six samples were stacked and shuffled; and each pad tested was conditioned by placing it at 23° C. in 50% relative humidity for five days prior to testing and using the methods outlined in ASTM D2240-15 (2015) to improve the repeatability of the hardness test. In the present invention, the Shore D hardness of the polyurethane reaction product of the polishing layer or pad includes the Shore D hardness of the reaction, which reaction includes any additives to increase the hardness. The term "Shore A" hardness refers to the same 15 second hardness measured with a larger A probe for a softer material.
[0033] As used herein, the term "solids" refers to any material that remains in the polyurethane reaction product of the present invention; thus, solids include reactive and nonvolatile liquids and additives that do not volatilize upon curing. Solids exclude water and volatile solvents.
[0034] As used herein, unless otherwise indicated, the term "viscosity" refers to the viscosity of a given material in pure form (100%) at a given temperature as measured using a rheometer set in an oscillatory shear rate sweep of 0.1-100 radians / second (in a 50 mm parallel plate geometry with a 100 μm gap).
[0035] As used herein, unless otherwise indicated, the term "wt. % NCO" refers to the amount of unreacted or free isocyanate groups in a given isocyanate or isocyanate-terminated urethane prepolymer composition.
[0036] As used herein, the term "wt. %" stands for weight percent.
[0037] According to the present invention, the inventors of the present invention have found that a CMP polishing pad having a high porosity CMP polishing layer with a hardness of> 40 Shore DO (15 seconds) is a useful hard pad having an attractive removal rate curve and capable of polishing with a low defect rate. In particular, a CMP polishing layer formed by spraying a reaction mixture having a hard segment weight fraction of 60wt.% to 68wt.%, or preferably higher than 60wt.%, provides a hard pad having a Shore DO (15 seconds) value higher than 40, or preferably at least 43 and a density lower than 0.50g / mL. CMP polishing pads within this hardness and porosity range were previously unavailable from other CMP production methods. In addition, the defect rate produced by using the CMP polishing pad of the present invention is unexpectedly good. Although the improved tensile modulus in the CMP polishing pad is considered to be a key driver of improved planarization efficiency (PE), the tensile modulus also increases the defects formed in CMP polishing.
[0038] The CMP polishing pad of the present invention is formed by a two-component reaction mixture having a liquid aromatic diisocyanate component and a liquid polyol component further containing the liquid aromatic diisocyanate component. The liquid aromatic diisocyanate component comprises one or more liquid aromatic diisocyanates or linear aromatic isocyanate-terminated urethane prepolymers. Suitable linear urethane prepolymers may be methylene diphenyl isocyanate (MDI) diisocyanate prepolymers having an NCO content greater than 18 wt.%; examples of such linear aromatic isocyanate-terminated urethane prepolymers include prepolymers formed from MDI and (di)ethylene glycol having an NCO content of 23.0 wt.% and an equivalent weight of 182 g / mol. Suitable reaction mixtures further comprise 0 to 25 wt.% (based on the total weight of the reaction mixture) of a liquid aromatic diamine as a curing agent. Liquid aromatic diamine curing agents contribute to fast reaction times and good mechanical properties of high tensile strength and high tensile modulus.
[0039] The hard segments of the reaction mixture ensure good mechanical properties.The hard segments may be 60 to 68 wt.% of the reaction mixture and may constitute part of both the polyol component and the aromatic isocyanate component.
[0040] As part of the hard segment of the reaction mixture, the diisocyanate is preferably methylene diphenyl diisocyanate (MDI), which is less toxic than toluene diisocyanate (TDI). The liquid aromatic isocyanate component may comprise a linear isocyanate-terminated urethane prepolymer formed from an extender or short chain diols like diols and diols, or preferably monoethylene glycol (MEG), dipropylene glycol (DPG) and / or tripropylene glycol (TPG).
[0041] Preferably, the liquid aromatic diisocyanate component contains only impurity levels of aliphatic isocyanates.
[0042] The soft segment of the reaction mixture may comprise a polymer polyol, such as a difunctional polyether in (ii) the polyol component. Suitable soft polyols are PTMEG and PPG. Useful examples of polyols containing PTMEG are as follows: Terathane from Invista, Wichita, KS. TM 2900, 2000, 1800, 1400, 1000, 650, and 250; Polymeg from Lyondell Chemicals, Limerick, PA TM 2900, 2000, 1000, 650; PolyTHF from BASF Corporation, Florham Park, NJ TM 650, 1000, 2000. Useful examples of PPG-containing polyols are as follows: Arcol from Covestro, Pittsburgh, PA. TM PPG-425, 725, 1000, 1025, 2000, 2025, 3025, and 4000; Voranol from Dow, Midland, MI TM 、Voralux TM , and Specflex TM Product line; each from Covestro (Leverkusen, DE) Multranol TM 、Ultracel TM 、Desmophen TM or Acclaim TM Polyol 12200, 8200, 6300, 4200, 2200.
[0043] The soft segment of the reaction mixture may also include one or more polyols having a polyether backbone and having 5 to 7 hydroxyl groups per molecule.
[0044] Suitable polyols having a polyether backbone and 5 to 7 hydroxyl groups per molecule are available as: VORANOL having 5 hydroxyl groups, a number average molecular weight of 590 and a hydroxyl value of 475 mg KOH / g TM 202 polyol (Dow), MULTRANOL with 6 hydroxyl groups, number average molecular weight of 3,366 and hydroxyl value of 100 mg KOH / g TM 9185 polyol (Dow), or VORANOL having an average of 6.9 hydroxyl groups, a number average molecular weight of 12,420, and a hydroxyl value of 31 mg KOH / g TM 4053 polyol (Dow).
[0045] The amount of ii) a) polymer polyol in the liquid polyol component may be an amount of up to 85 wt. % of the liquid polyol component.
[0046] The liquid aromatic diamine curing agent of the present invention may account for 0 to 25 wt.%, or preferably 0 to 20 wt.%, based on the total solid weight of the reaction mixture.
[0047] Suitable curing agents are aromatic diamines which are liquid at standard pressure and 40°C. However, the curing agent must be slow enough to allow mixing of the two-component reaction mixture. When combined with the aromatic isocyanate component and the polyol component, the curing agent must cause gelation (so that the reactive mixture combination no longer flows) for at least 15 seconds, or preferably at least 20 seconds. Therefore, the curing agent of the present invention does not contain more than 5 wt.% of N,N-primary alkylaryl diamine or N,N-secondary or tertiary alkyl diamine as solids.
[0048] In order to increase the reactivity of the polyol component with diisocyanates or polyisocyanates, a catalyst may be used. Suitable catalysts include any catalyst known to those skilled in the art, such as oleic acid, azelaic acid, dibutyltin dilaurate, tin octoate, bismuth octoate, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), tertiary amine catalysts such as Dabco TM TMR catalyst, triethylenediamine such as DABCO TM 33LV, and mixtures thereof. Amine catalysts can accelerate the foaming reaction.
[0049] The reaction mixture of the present invention is substantially free of added organic solvents.
[0050] The specific gravity of the resulting CMP polishing pad is 0.2 to 0.5, preferably 0.35 to 0.495. As the porosity increases, the bulk properties of the CMP polishing pad decrease, and the removal rate (RR) increases. However, when the CMP polishing pad or layer exhibits increased porosity and is a hard layer or pad, the defect rate and planarization efficiency are not expected to improve.
[0051] The CMP polishing pad or layer of the present invention comprises a large number average pore size (X 50 ) (75 to 200 microns, or preferably 80 to 140 microns as determined by scanning electron microscopy (SEM). The stoichiometry of the reaction mixture of the present invention is (NH+OH):NCO 0.85:1.0 to 1.15:1.0.
[0052] The chemical mechanical polishing layer or pad of the present invention comprises a polishing layer which is a uniform dispersion of porous polyurethane. Uniformity is important for obtaining consistent polishing pad performance. Therefore, the reaction mixture of the present invention is selected so that the resulting pad morphology is stable and easily reproducible. For example, control of additives such as antioxidants and impurities such as water is generally important for consistent manufacturing.
[0053] According to the present invention, the CMP polishing layer can be made by spraying the reaction mixture onto an open mold and curing it. Because the two-component reaction mixture of the present invention can be sprayed or deposited as a fluid to make the CMP polishing layer, the reaction mixture of the present invention can react much faster than when such a layer is formed in a closed mold. The gel time of the reaction mixture at 65° C. is 10 seconds or more, or preferably 15 seconds to 2 minutes.
[0054] The liquid reaction mixture of the present invention can comprise a very fast curing composition in which the (i) liquid aromatic isocyanate component and (ii) liquid polyol component can gel in a gel time as short as 15 seconds. The reaction must be slow enough so that the reaction mixture can be mixed in a static or impingement mixer after combining the two components. One limitation of the gel time is that the reaction mixture must react slowly enough so as not to clog the mixing head in which it is mixed and to properly fill the mold when it is applied to the mold surface.
[0055] Preferably, the target or substrate in the method of the present invention is an open mold, wherein the produced pad will have a directly bonded groove pattern.
[0056] The CMP polishing layer of the present invention can be produced by impingement mixing or static mixing of a reaction mixture in combination with a blowing agent such as water or CO2 amine (carbamate) (e.g., CO2 alkanolamine blowing agent). After impingement or static mixing, the reactive mixture is sprayed from a nozzle toward a target in an air-induced or airless spray. In this way, polyurethane or polyurethane-urea CMP polishing layers with variable porosity of 0.1 g / mL to 0.5 g / mL can be obtained in a controlled process with good uniformity of substantially spherical pores throughout the pad.
[0057] The fast gel time of the reaction mixture of the present invention means that the pores formed during spraying or deposition will remain in the cured CMP polishing layer. Therefore, surfactants, such as nonionic surfactants (such as polyethoxylated siloxanes), are not required in the reaction mixture of the present invention to produce stable foam articles therefrom.
[0058] Furthermore, since the CMP polishing pad of the present invention is formed by spraying or foaming in the presence of a foaming agent to form a foam, trace elements such as hollow microspheres are not required, and preferably are absent.
[0059] Porosity is introduced into the pad or polishing layer by spraying, and the resulting pad tensile modulus is a function of both the intrinsic polymer tensile modulus and the porosity, with the increased porosity acting to reduce the density or specific gravity. Thus, for a two-component spray-made pad or polishing layer, in order to provide an acceptable tensile modulus, the polymer matrix tensile modulus must be acceptably high, preferably greater than 344 MPa and more preferably greater than 482 MPa.
[0060] Polishing layer or pad density is measured according to ASTM D1622-08 (2008). Density is the same as specific gravity.
[0061] The CMP polishing layer or pad of the present invention is effective for interlayer dielectric (ILD) and inorganic oxide polishing. For the purpose of the present invention, removal rate refers to the removal rate in Represents the removal rate.
[0062] The chemical mechanical polishing pad of the present invention may comprise only a polishing layer of a polyurethane reaction product or a polishing layer stacked on a subpad or sublayer. The polishing pad, or in the case of a stacked pad, the polishing layer of the polishing pad of the present invention may be used in both porous and non-porous, or unfilled configurations.
[0063] Preferably, the polishing layer used in the chemical mechanical polishing pad of the present invention has an average thickness of 500 to 3750 microns (20 to 150 mils), or more preferably 750 to 3150 microns (30 to 125 mils), or still more preferably 1000 to 3000 microns (40 to 120 mils), or most preferably 1250 to 2500 microns (50 to 100 mils).
[0064] The chemical mechanical polishing pad of the present invention optionally further comprises at least one additional layer interfacing with the polishing layer. Preferably, the chemical mechanical polishing pad optionally further comprises a compressible subpad or foundation layer adhered to the polishing layer. The compressible foundation layer preferably improves the conformity of the polishing layer to the surface of the substrate being polished.
[0065] The polishing layer of the chemical mechanical polishing pad of the present invention has a polishing surface adapted to a polishing substrate. Preferably, the polishing surface has a macro texture selected from at least one of holes and grooves. The holes can extend partially from the polishing surface or extend all the way through the thickness of the polishing layer.
[0066] Preferably, the grooves are arranged on the polishing surface such that when the chemical mechanical polishing pad is rotated during polishing, at least one groove sweeps across the surface of the substrate being polished.
[0067] Preferably, the polishing layer of the chemical mechanical polishing pad of the present invention has a polishing surface adapted to a polishing substrate, wherein the polishing surface has a macrotexture comprising a groove pattern formed therein and selected from curved grooves, linear grooves, perforations, and combinations thereof. Preferably, the groove pattern comprises a plurality of grooves. More preferably, the groove pattern is selected from a groove design, such as a groove design selected from the group consisting of concentric grooves (which may be circular or spiral), curved grooves, mesh grooves (e.g., arranged as an XY grid on the pad surface), other regular designs (e.g., hexagonal, triangular), tire tread type patterns, irregular designs (e.g., fractal patterns), and combinations thereof. More preferably, the groove design is selected from the group consisting of random grooves, concentric grooves, spiral grooves, mesh grooves, XY grid grooves, hexagonal grooves, triangular grooves, fractal grooves, and combinations thereof. Most preferably, the polishing surface has a spiral groove pattern formed therein. The groove profile is preferably selected from a rectangle with straight sidewalls, or the groove cross section may be "V", "U", serrated, and combinations thereof.
[0068] According to the method of making a polishing pad according to the present invention, the chemical mechanical polishing pad can be molded with a macrotexture or groove pattern in its polishing surface to promote slurry flow and remove polishing debris from the pad-wafer interface. Such grooves can be formed in the polishing surface of the polishing pad by the shape of the mold surface, that is, where the mold has a negative topographical form of the macrotexture.
[0069] The chemical mechanical polishing pad of the present invention can be used for polishing at least one substrate selected from the group consisting of a magnetic substrate, an optical substrate, and a semiconductor substrate.
[0070] Preferably, the method for polishing a substrate of the present invention comprises: providing a substrate selected from at least one of a magnetic substrate, an optical substrate and a semiconductor substrate (preferably a semiconductor substrate, such as a semiconductor wafer); providing a chemical mechanical polishing pad according to the present invention; generating dynamic contact between the polishing surface of the polishing layer and the substrate to polish the surface of the substrate; and conditioning the polishing surface with an abrasive conditioner.
[0071] Conditioning the polishing pad includes bringing a conditioning disk into contact with the polishing surface when polishing is paused ("ex-situ") or during intermittent breaks in the CMP process while the CMP process is ongoing ("in-situ"). The conditioning disk has a rough conditioning surface that typically includes embedded diamond points that cut microscopic grooves in the pad surface, grinding and scoring the pad material and renewing the polishing texture. Typically, the conditioning disk rotates in a fixed position relative to the rotational axis of the polishing pad and sweeps over an annular conditioning area as the polishing pad rotates.
[0072] Examples: The present invention will now be described in detail in the following non-limiting examples:
[0073] Unless otherwise indicated, all temperatures are room temperature (21-23° C.) and all pressures are atmospheric pressure (approximately 760 mm Hg or 101 kPa).
[0074] The following raw materials were used in the examples, although there are other raw materials disclosed below:
[0075] Ethacure TM 300 Curing Agent: dimethylthiotoluenediamine (DMTDA), an aromatic diamine (Albemarle, Charlotte, NC).
[0076] Voranol TM V5055HH polyol: multifunctional polyether polyol (OH equivalent weight 2000), functionality = 6, with a number average molecular weight M of 12,000 N High molecular weight ethylene oxide terminated propylene oxide polyol (The Dow Chemical Company, Midland, MI).
[0077] MDI prepolymer: a linear isocyanate-terminated urethane prepolymer from MDI and small molecule dipropylene glycol (DPG) and tripropylene glycol (TPG), having an NCO content of about 23 wt.% and an equivalent weight of 182. 100 wt.% of this MDI prepolymer was regarded as a hard segment.
[0078] Niax TM L5345 surfactant: nonionic silicone surfactant (Momentive, Columbus, OH).
[0079] DABCO made from diazabicyclononane (triethylenediamine) TM 33LV amine catalyst (Air Products, Allentown, PA), DABCO 33LV is a blend of 33 wt.% triethylenediamine and 67 wt.% dipropylene glycol.
[0080] PTMEG####: Poly(THF) or polytetramethylene glycol, prepared by ring-opening polymerization of tetrahydrofuran (THF) and used as PolyTHF TM Polyols are sold as PolyTHF from BASF, Leverkusen, DE. The number after PTMEG is the average molecular weight as reported by the manufacturer. The polyols are commercially available from BASF (as PolyTHF TM PolyTHF is sold as PolyTHF 650 (PolyTHF 650, PolyTHF 1000, PolyTHF 2000) and is available in three different grades of molecular weight 650, 1000 or 2000.
[0081] Niax TM T-9 catalyst: stannous octoate (Momentive).
[0082] CMP pad properties were evaluated according to the following methods:
[0083] All tensile properties were measured according to ASTM D412-06a, "Standard Test Methods for Vulcanized Rubber and Thermoplastic Elastomers—Tension". Samples were cut into dog-bone C dimensions. Five test specimens were measured, and the average of all test specimens for each analyte sample was reported, unless otherwise specified.
[0084] Tensile elongation at break:It means the ratio between the changed length after the test specimen breaks and the initial length, and is tested according to ASTM D412-06a (2006), "Standard Test Methods for Vulcanized Rubber and Thermoplastic Elastomers - Tension".
[0085] In all of the following examples, the specified two-component reaction mixture was mixed and sprayed onto an open mold using an impingement mix and air spray system with two tanks (isocyanate (iso) tank and polyol (poly) tank) to feed the mixing system. The two tanks were set at a given material flow rate, from which the relative amounts of each of the two components were easily determined. Flow from both tanks was started and stopped simultaneously.
[0086] Comparative Example 1: The reaction mixture was sprayed into an open mold using a two-component impingement mixing and air spraying system. The isocyanate (iso) tank was filled with MDI prepolymer, while the polyol (poly) tank was filled with 98.62 parts of PolyTHF650, 0.9857 parts of Niax TM L5345 nonionic surfactant, 0.09857 parts Niax TM T-9 catalyst, 0.2957 parts of DABCO 33LV catalyst. The flow rate on the polyol side during spraying was 10.11 g / s, and the flow rate on the isocyanate (iso) side was 5.89 g / s. The air injected into the nozzle was set to a nominal rate of 100 L / min. The sprayed polyurethane formulation was directed onto a polytetrafluoroethylene (PTFE) coated aluminum plate. The sprayed pad was cured in a 100°C oven for 16 hours. The resulting polishing layer had a 37 wt.% hard segment weight fraction at 95% stoichiometry without added water, and produced a single-layer pad having a bulk density of 0.88 g / mL and exhibiting a bulk tensile modulus of 1.37 MPa, a tensile strength of 3.10 MPa, a tensile elongation of 1300%, and a 15-second Shore A hardness of 35.
[0087] Comparative Example 2: The reaction mixture was sprayed into an open mold using a two-component impingement mixing and air spraying system. The isocyanate tank was filled with MDI prepolymer, while the polyol tank was filled with 98.62 parts of PolyTHF650, 0.9857 parts of Niax TM L5345 nonionic surfactant, 0.09857 parts Niax TMT-9 catalyst, 0.2957 parts of DABCO 33LV catalyst. The flow rate on the polyol side during spraying is 10.11 g / s, and the flow rate on the isocyanate (iso) side is 5.89 g / s. The air injected into the nozzle is set to a nominal rate of 20 L / min. The sprayed polyurethane formulation is directed onto a PTFE-coated aluminum plate. The sprayed pad is cured in a 100 ° C oven for 16 hours. The resulting pad is described as a 37 wt.% hard segment weight fraction at 95% stoichiometry without added water, and produces the following pad, which has a bulk density of 0.97 g / mL and shows a bulk tensile modulus of 1.65 MPa, a tensile strength of 3.65 MPa, and a tensile elongation of 1200%, and a 15-second Shore A hardness of 36.
[0088] Comparative Example 3: The reaction mixture was sprayed into an open mold using a two-component impingement mixing and air spraying system. The isocyanate tank was filled with MDI prepolymer, while the polyol tank was filled with 98.52 parts of PolyTHF650, 0.9847 parts of Niax TM L5345 nonionic surfactant, 0.09847 parts Niax TM T-9 catalyst, 0.2954 parts of DABCO 33LV catalyst and 0.098 parts of water. The flow rate of the polyol side during spraying is 9.99g / s, and the flow rate of the isocyanate (iso) side is 6.01g / s. The air injected into the nozzle is set to a nominal rate of 100L / min. The sprayed polyurethane formulation is directed onto a Teflon-coated aluminum plate. The sprayed pad is cured in a 100°C oven for 16 hours. The resulting pad is described as a 38wt.% hard segment weight fraction at 95% stoichiometry with the addition of 1000ppm of water, and produces the following pad, which has a bulk density of 0.73g / mL and shows a bulk tensile modulus of 1.03MPa (150psi), a tensile strength of 3.65MPa (530psi) and a tensile elongation of 1200%, and a 15-second Shore A hardness of 32.
[0089] Comparative Example 4: The reaction mixture was sprayed into an open mold using a two-component impingement mixing and air spraying system. The isocyanate tank was filled with MDI prepolymer, while the polyol tank was filled with 98.52 parts of PolyTHF650, 0.9847 parts of Niax TM L5345 nonionic surfactant, 0.09847 parts Niax TMT-9 catalyst, 0.2954 parts of DABCO 33LV catalyst and 0.098 parts of water. The flow rate of the polyol side during spraying is 9.99g / s, and the flow rate of the isocyanate (iso) side is 6.01g / s. The air injected into the nozzle is set to a nominal rate of 20L / min. The sprayed polyurethane formulation is directed onto a Teflon-coated aluminum plate. The sprayed pad is cured in a 100°C oven for 16 hours. The resulting pad is described as a 38wt.% hard segment weight fraction at 95% stoichiometry with the addition of 1000ppm of water, and produces the following pad, which has a bulk density of 0.80g / mL and shows a bulk tensile modulus of 1.31MPa (190psi), a tensile strength of 3.72MPa (540psi) and a tensile elongation of 1200%, and a 15-second Shore A hardness of 33.
[0090] Comparative Example 5: The reaction mixture was sprayed into an open mold using a two-component impingement mixing and air spray system. The MDI prepolymer was loaded into the isocyanate tank, while 98.18 parts of PolyTHF650, 0.9814 parts of Niax L5345 nonionic surfactant, 0.0986 parts of Niax T-9 catalyst, 0.2942 parts of DABCO 33LV and 0.441 parts of water were loaded into the polyol tank. The flow rate on the polyol side during spraying was 9.56 g / s, and the flow rate on the isocyanate (iso) side was 6.44 g / s. The air injected into the nozzle was set to a nominal rate of 100 L / min. The sprayed polyurethane formulation was directed onto a Teflon-coated aluminum plate. The sprayed pad was cured in a 100° C. oven for 16 hours. The resulting pad is described as 40.7 wt.% hard segment weight fraction at 95% stoichiometry and with the addition of 4500 ppm water, and produces a pad having a bulk density of 0.39 g / mL and exhibiting a bulk tensile modulus of 0.455 MPa (66 psi), a tensile strength of 1.93 MPa (280 psi), and a tensile elongation of 890%, with a 15 second Shore A hardness of 15.
[0091] Comparative Example 6:The reaction mixture was sprayed into an open mold using a two-component impingement mixing and air spraying system. MDI prepolymer was loaded into the isocyanate tank, while 87.99 parts of PolyTHF650, 0.88 parts of Niax L5345 nonionic surfactant, 0.0886 parts of Niax T-9 catalyst, 0.264 parts of DABCO 33LV and 0.220 parts of water and 10.557 parts of dipropylene glycol were loaded into the polyol tank. The flow rate on the polyol side during spraying was 8.57 g / s, and the flow rate on the isocyanate (iso) side was 7.43 g / s. The air injected into the nozzle was set to a nominal rate of 100 L / min. The sprayed polyurethane formulation was directed onto a Teflon-coated aluminum plate. The sprayed pad was cured in a 100° C. oven for 16 hours. The resulting pad is described as 52.5 wt. % hard segment weight fraction at 95% stoichiometry and with the addition of 2500 ppm water, and produces a pad having a bulk density of 0.53 g / mL and exhibiting a bulk tensile modulus of 1.17 MPa (170 psi), a tensile strength of 6.00 MPa (870 psi), and a tensile elongation of 535%, with a 15 second Shore A hardness of 27.
[0092] Example 7: The reaction mixture was sprayed into an open mold using a two-component impingement mixing and air spraying system. The MDI prepolymer was loaded into the isocyanate tank, while 73.179 parts of PolyTHF650, 0.7316 parts of Niax L5345 nonionic surfactant, 0.0734 parts of Niax T-9 catalyst, 0.2189 parts of DABCO 33LV and 0.183 parts of water and 25.6126 parts of dipropylene glycol were loaded into the polyol tank. The flow rate on the polyol side during spraying was 7.26 g / s, and the flow rate on the isocyanate (iso) side was 8.74 g / s. The air injected into the nozzle was set to a nominal rate of 100 L / min. The sprayed polyurethane formulation was directed onto a Teflon-coated aluminum plate. The sprayed pad was cured in a 100° C. oven for 16 hours. The resulting one layer mat is described as 66 wt.% hard segment weight fraction at 95% stoichiometry and with the addition of 2500 ppm water, and produces a mat having a bulk density of 0.49 g / mL and exhibiting a bulk tensile modulus of 207 MPa (30,100 psi), a tensile strength of 7.58 MPa (1,100 psi) and a tensile elongation of 66%, a 15 sec Shore A hardness of 82, and a Shore DO (15 sec) hardness of 60.
[0093] Polishing experiments were performed on 200 mm wafers on an Applied Mirra polisher (Applied Materials, Santa Clara, CA) with carrier downforces of 0.014, 0.016, 0.021, and 0.026 MPa (2.0, 2.3, 3.0, and 3.8 psi), a slurry flow rate of 200 mL / min, and Klebosol TM II1730 colloidal silica slurry (Dow, 16 wt.% solids), the table rotation speed was 93 rpm, and the carrier rotation speed was 87 rpm. 3M TM A diamond pad conditioner A153L (108 mm (4.25 in) diameter, 3M aggressiveness grade 6-9 (The 3M Company, Minneapolis, MN)) was used to condition and texture the polishing pad. The polishing pads were each broken in with the conditioner and DI water using only a down force of 22.2 N for 30 min. The polishing pad was further 100% conditioned in situ during polishing at 10 scans / min with a down force of 22.2 N from 43 to 234 mm (1.7 to 9.2 in) from the center of the polishing pad. The polishing pad was then subjected to a 30 min in-situ polishing cycle ... TM The wafers were cleaned on a post-CMP cleaner (Lam Research, Fremont, CA). To further highlight shallow scratches, 200 Ang of TEOS was etched from the wafer by hydrogen fluoride (HF) etching on a SSEC single wafer etch system (Veeco, Horsham, PA). Planarized step height measurements were performed on a Bruker dynamic atomic force profiler (Bruker, Billerica, MA). The substrate was a tetraethoxysilicate (TEOS) wafer substrate. The 3D images were taken using a KLA-Tencor FX200 TM The metrology tool (KLA Tencor, Milpitas, CA) used a 49-point spiral scan to measure the film thickness before and after polishing at 3 mm edge exclusion to determine Removal rate The removal rate (in angstroms per minute) was calculated from the change in thickness at each point during a specified polishing time.
[0094] Inhomogeneity ratio The (%NUR) is calculated by the % standard deviation of the removal rate.
[0095] Defect Rate Using SP2 XP TM and eDR5210 TM Determined by scanning electron microscope wafer defect inspection system (Klarity Corporation). TM The software manually classifies defect types from a randomly selected set of 100 defects.
[0096] Defects are categorized as follows:
[0097] A-HF etches anything the computer sees before; and,
[0098] Anything the computer sees after the B-HF etch; and
[0099] C - Chatter scratches identified by visual inspection by trained personnel. The polishing results are given in Table 1 below.
[0100] Table 1: Pad properties
[0101]
[0102] The removal rate curves are given in Table 1 above, showing the relationship between IC1000 and TM 7% higher removal rate compared to pads. The wafers were imaged directly after DI water rinse and drying after polishing. IC1000 TM The average number of defects after polishing of the pad was 405, while Example 7 produced an average of 302 defects. Thus, the inventive pad of Example 7 showed slightly improved removal rate and greater pad hardness, but with significantly fewer defects during polishing. It is expected that a more porous pad with a lower density (less than 0.49 g / mL) would not be as hard and would provide even better defectivity performance.
Claims
1. A chemical mechanical (CMP) polishing pad for polishing a substrate, wherein the substrate is selected from at least one of a magnetic substrate, an optical substrate and a semiconductor substrate, characterized in that: The polishing pad comprises a polishing layer adapted to polish the substrate, the polishing layer being a polyurethane which is the product of a two-component reaction mixture free of organic solvents comprising: (i) a liquid aromatic isocyanate component comprising one or more aromatic diisocyanates or linear aromatic isocyanate-terminated urethane prepolymers having an unreacted isocyanate (NCO) concentration of 18 to 40 wt.%, based on the total solid weight of the aromatic isocyanate component, and (ii) a liquid polyol component comprising a) one or more polymer polyols, b) 15 to 36 wt.% of a polyol having 2 to 6 isocyanates, based on the total weight of the liquid polyol component. % of a small chain difunctional polyol having carbon atoms, c) 0 to 25 wt.% of a liquid aromatic diamine, based on the total weight of the liquid polyol component, the liquid aromatic diamine being liquid at standard pressure and 40° C., and d) water or a CO2-amine adduct in an amount sufficient to reduce the density of a CMP polishing pad made from the two-component reaction mixture to 0.2 to 0.50 g / mL, wherein the reaction mixture contains 60 to 75 wt.% of a hard segment material, based on the total weight of the reaction mixture, wherein the CMP polishing layer has a Shore DO hardness of 40 to 80 at 15 seconds and has a density of 0.2 to 0.50 g / mL.
2. The CMP polishing pad according to claim 1, wherein The (i) liquid aromatic isocyanate component comprises one or more diisocyanates or isocyanate-terminated linear urethane prepolymer compounds selected from the group consisting of methylene diphenyl diisocyanate (MDI), toluene diisocyanate (TDI), naphthalene diisocyanate (NDI), p-phenylene diisocyanate (PPDI), or o-toluidine diisocyanate (TODI); linear isocyanate-terminated urethane prepolymers of any one of MDI, TDI, NDI, PPDA, TODI extended with one or more extender compounds, or mixtures thereof; or mixtures thereof.
3. The CMP polishing pad according to claim 2, wherein: The (i) liquid aromatic isocyanate component is selected from methylene diphenyl diisocyanate (MDI) or a linear isocyanate-terminated urethane prepolymer of MDI, wherein the prepolymer is MDI or an MDI dimer extended with any one of the following: ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, tripropylene glycol and mixtures thereof.
4. The CMP polishing pad according to claim 1, wherein In the (ii) liquid polyol component, the one or more polymer polyols are selected from polytetramethylene glycol (PTMEG), polypropylene glycol (PPG), hexafunctional polyols, and mixtures thereof.
5. The CMP polishing pad according to claim 1, wherein In the (ii) liquid polyol component, the one or more small-chain difunctional polyols having 2 to 6 carbon atoms are selected from ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 2-methyl-1,3-propylene glycol, 1,4-butylene glycol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, and mixtures thereof.
6. The CMP polishing pad according to claim 5, wherein: In the (ii) liquid polyol component, the one or more small-chain difunctional polyols having 2 to 6 carbon atoms are selected from ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol and mixtures thereof.
7. The CMP polishing pad according to claim 1, wherein: The reaction mixture comprises greater than 63 to 75 wt. % hard segment material.
8. The CMP polishing pad according to claim 1, wherein: The stoichiometric ratio of the sum of the total moles of amine (NH2) groups and the total moles of hydroxyl (OH) groups in the reaction mixture to the total moles of unreacted isocyanate (NCO) groups in the reaction mixture for producing the CMP polishing layer is 0.85:1.0 to 1.15:1.
0.
9. The CMP polishing pad according to claim 1, wherein: The CMP polishing pad contains no trace elements other than those formed from the water or CO2-amine adducts.
10. The CMP polishing pad according to claim 1, wherein: d) is water, the amount of water is 1,000 and 8,500 ppm based on the total weight of the two-component reaction mixture.