A catalytic cracking aid and its preparation method and application
By using a catalytic cracking additive combined with alumina and high stability matrix in the catalytic cracking catalyst, the problems of reduced catalyst activity and resource waste are solved, the propylene yield and the anti-wear properties of the catalyst are significantly improved, and the glue slag is realized recycling.
Patent Information
- Application Number
- CN202111275286.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-29
AI Technical Summary
When aluminum phosphate sol is used as a binder in existing catalytic cracking catalysts, the activity of the catalyst is reduced, and the slag in the catalyst production cannot be effectively recovered, resulting in waste of resources.
Using catalytic cracking additives containing alumina and high stability matrix, the slag is finely ground and reacted with an aluminum source to form a high stability matrix and combine it with an alumina binder for the preparation of catalytic cracking with high cracking activity. Additive.
The concentration of propylene in the liquefied gas is significantly improved, the high activity and wear resistance of the catalyst are achieved, and the resource recycling of the glue slag is achieved.
Smart Images

Figure BDA0003329856900000111 
Figure BDA0003329856900000112 
Figure BDA0003329856900000121
Abstract
Description
Technical Field
[0001] The invention relates to a catalytic cracking aid and a preparation method and application thereof. Background Art
[0002] Catalytic cracking is one of the important production processes for light olefins. Using a catalyst or additive containing MFI zeolite is an effective method. MFI zeolite can selectively crack C6~C 12 Alkanes and alkenes can generate C3-C5 olefins and increase the yield of low-carbon olefins.
[0003] The catalytic cracking catalyst or auxiliary agent for increasing the production of propylene disclosed in the prior art mainly modifies the ZSM-5 molecular sieve, but the adhesive matrix ensures the anti-wear performance of the catalyst and can synergize with the active components of the molecular sieve to improve the activity and hydrothermal stability of the catalyst. USP 3544476 discloses a method for preparing a water treatment agent containing phosphorus and aluminum: adding metal aluminum powder to a hydrochloric acid solution, reacting at 90°C for 2 hours, then adding phosphoric acid, and then aging at 80°C for 30 minutes. CN1417296A provides a method of beating and dispersing an acid-soluble aluminum hydroxide or aluminum oxide with decationized water into a slurry with a solid content of 15 to 35% by weight, adding concentrated phosphoric acid to the slurry at a weight ratio of P / Al=1.2 to 6 under stirring, and then heating to 65 to 95°C, and reacting at this temperature for 15 to 90 minutes until it becomes a transparent colloid. The preparation method of aluminum phosphate sol provided by CN102050434A comprises: slurrying and dispersing an acid-soluble aluminum precursor and decationized water into a slurry with a solid content of 10 to 35 weight percent, adding phosphoric acid with a concentration of 60 to 98 percent according to a weight ratio of P / Al=1.0 to 2.5 and adding nitric acid with a concentration of 40 to 98 percent according to a weight ratio of HNO3 / Al2O3=0.2 to 2.0 to the slurry under stirring, and obtaining aluminum phosphate sol after the reaction.
[0004] The use of this phosphorus-containing aluminum sol as a binder may cause the molecular sieve to block the pores, thereby affecting the activity of the catalyst.
[0005] The catalyst matrix should have a large pore size, suitable activity and good hydrothermal stability, so that the catalyst can withstand harsh hydrothermal operating conditions and pre-cracking heavy crude oil. The slag is a waste residue with Al2O3 and SiO2 as the main components, obtained by sedimentation, filtration and slag cutting of wastewater generated in the production of catalytic cracking catalysts, and also contains 2% to 15% Na2O and 1% to 15% RE2O3. At present, the slag is mainly discarded directly, resulting in a waste of resources such as Si and Al. Summary of the invention
[0006] The purpose of the present invention is to provide a catalytic cracking aid for increasing the concentration of propylene, and a preparation method and application thereof. The catalytic cracking aid of the present invention has high cracking activity and can significantly increase the concentration of propylene in liquefied gas.
[0007] According to one aspect of the present invention, there is provided a catalytic cracking aid, which comprises, based on the total weight of the catalytic cracking aid, (1) 15 to 55 wt% of a zeolite having an MFI structure; (2) 2 to 20 wt% of an alumina binder; (3) 10 to 50 wt% of a high stability matrix, which comprises, based on the total weight of the high stability matrix, 0.1 to 10.0 wt% of Na2O, 5 to 35 wt% of Al2O3, 5 to 25 wt% of SiO2, 30 to 80 wt% of P2O5, and 1 to 10 wt% of RE2O3; and (4) 10 to 50 wt% of clay.
[0008] According to another aspect of the present invention, the present invention provides a method for preparing a catalytic cracking aid, which includes preparing a highly stable matrix; the highly stable matrix is prepared by the following steps: 1) slurrying the slurry uniformly, with a solid content of 10 to 20% by weight, and grinding; 2) adding acid to the ground slurry, adjusting the pH to 2 to 5, heating to 70-150° C. for constant temperature reaction for 30-150 minutes, and then cooling to 10 to 50° C. to activate the slurry once; 3) stirring the ground slurry uniformly with an aluminum source; 4) adding concentrated phosphoric acid to control the total solid content of the slurry to be 25 to 45% by weight; 4) reacting the obtained slurry at 50 to 95° C. for 60 to 150 minutes and then cooling to 10 to 50° C.; the pH value of the slurry is 0.5 to 3.5, i.e., a highly stable matrix; wherein the weight ratio of the slurry to the aluminum source is 0.1 to 30:1, and the weight of the aluminum source is calculated as alumina; the above step 2) is an optional step.
[0009] According to some embodiments of the present invention, based on the dry weight of the slag, the slag contains 10-50 wt % Al2O3, 30-70 wt % SiO2, 2-15 wt % Na2O and 1-15 wt % RE2O3.
[0010] According to some embodiments of the present invention, the particle size of the slag is controlled to be D(V, 0.5) ≤ 5 μm, D(V, 0.9) ≤ 15 μm.
[0011] According to some embodiments of the present invention, the acid in step 2) may be one or a mixture of two or more of phosphoric acid, nitric acid, sulfuric acid, and an organic acid.
[0012] According to some embodiments of the present invention, the aluminum source is selected from one or more of pseudo-boehmite, aluminum hydroxide, aluminum sol, aluminum nitrate, aluminum chloride, and aluminum sulfate.
[0013] According to some embodiments of the present invention, the method further comprises the steps of spray drying, calcining and washing after mixing water, zeolite having an MFI structure, a highly stable matrix, an alumina binder and clay. The steps comprise:
[0014] (1) mixing water, clay and alumina binder and beating to obtain a first slurry;
[0015] (2) mixing and beating the first slurry, the zeolite having an MFI structure and the high-stability matrix to obtain a second slurry; and
[0016] (3) The obtained second slurry is spray-dried, calcined and washed.
[0017] According to some embodiments of the present invention, the solid content of the first slurry and the second slurry is 20-40% by weight.
[0018] According to some embodiments of the present invention, the alumina binder is selected from one or both of pseudo-boehmite and alumina sol.
[0019] According to some embodiments of the present invention, the zeolite with MFI structure is selected from ZSM-5 zeolite; the clay is selected from one or more of kaolin, rectorite, diatomite, montmorillonite, bentonite and sepiolite. The ZSM-5 zeolite is selected from HZSM-5 zeolite and / or modified ZSM-5 zeolite, and the modified ZSM-5 zeolite contains one or more of phosphorus, iron and rare earth metals.
[0020] According to some embodiments of the present invention, in the method for preparing the catalytic cracking aid, the spray drying tower temperature is 120-200°C.
[0021] According to some embodiments of the present invention, in the method for preparing the catalytic cracking aid, the calcination temperature is 260-550°C.
[0022] According to some embodiments of the present invention, in the preparation method of the catalytic cracking aid, the washing method includes: exchange washing with one or more of dilute phosphoric acid, dilute hydrochloric acid, dilute sulfuric acid, dilute nitric acid, and ammonium salts, the washing temperature is room temperature to 80°C, the washing time is 10 to 60 minutes, and the pH is 0.5-6.
[0023] According to another aspect of the present invention, the present invention provides the use of the above-mentioned catalytic cracking aid in catalytic cracking of crude oil.
[0024] According to another aspect of the present invention, the present invention provides a catalytic cracking method, which comprises the step of contacting hydrocarbon oil with the catalytic cracking aid of the present invention for reaction.
[0025] According to some embodiments of the present invention, the catalytic cracking method of the present invention comprises the step of reacting hydrocarbon oil with the catalytic cracking aid of the present invention and a main catalyst. The main catalyst is a catalyst conventionally used in the catalytic cracking reaction of hydrocarbon oil, including but not limited to vanadium-resistant catalytic cracking catalyst RCGP, iron-resistant catalytic cracking catalyst CMT-1, high-activity heavy oil cracking catalyst HAC, high-yield diesel catalytic cracking catalyst MLC500, etc.
[0026] According to some embodiments of the present invention, in the application, the conditions for catalytic cracking of crude oil include: a temperature of 490-530° C. and a catalyst-to-oil ratio of 3-8.
[0027] According to some embodiments of the present invention, in the application, the content of the catalytic cracking aid is 1 to 50 wt % based on the total weight of the catalytic cracking aid and the catalytic cracking catalyst.
[0028] The catalytic cracking aid of the present invention contains a highly stable matrix prepared from the slag, which not only realizes the recycling of the slag but also enables the catalytic cracking aid to have better cracking activity and can effectively increase the concentration of propylene in the liquefied gas.
[0029] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0030] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0031] The first aspect of the present invention provides a catalytic cracking aid. Based on the total weight of the catalytic cracking aid, the catalytic cracking aid comprises:
[0032] (1) 15 to 55 wt% of ZSM-5 zeolite; (2) 2 to 20 wt% of alumina binder; (3) 10 to 50 wt% of a high-stability matrix, based on the total weight of the high-stability matrix, containing 0.1 to 10.0 wt% of Na2O, 5 to 35 wt% of Al2O3, 5 to 25 wt% of SiO2, 30 to 80 wt% of P2O5, and 1 to 10 wt% of RE2O3. (4) 10 to 50 wt% of clay. Among them, RE2O3 refers to rare earth metal oxides, which are well known to those skilled in the art and will not be described in detail here. The high-stability matrix of the present invention contains slag, which not only realizes the effective recycling of resources such as silicon, aluminum, and rare earth in the catalyst production process, but also has a high cracking activity and can significantly increase the concentration of propylene in liquefied gas.
[0033] Based on the total weight of the high-stability matrix, it contains 0.1-10.0 wt% Na2O, 5-35 wt% Al2O3, 5-25 wt% SiO2, 30-80 wt% P2O5, and 1-10 wt% RE2O3. (4) 10-50 wt% clay. The catalytic cracking aid of the present invention uses alumina and the high-stability matrix as binders at the same time. Compared with conventional aluminum phosphate sol, the high-stability matrix has a stable aluminum phosphate colloidal system and contains a certain amount of silicon aluminum fragments and rare earth in the matrix. While ensuring that the catalytic cracking aid has good anti-wear ability, it also has a higher specific surface area and cracking activity. When the catalytic cracking aid of the present invention is used in a catalytic cracking reaction, the concentration of propylene in the liquefied gas can be significantly increased, the yield of liquefied gas can be increased, and a higher total conversion rate and gasoline yield can be ensured. The alumina binder used in the present invention and the high-stability matrix prepared by the present invention both have bonding properties. When used as a binder together, the matrix has a higher macromolecular cracking performance. The high-stability matrix also has a silicon-aluminum or silicon-aluminum-phosphorus structure. The high-stability matrix with this structure is used in combination with an alumina binder, which can improve the activity of the matrix while ensuring that the catalyst has good anti-wear performance.
[0034] According to the present invention, the catalytic cracking aid may contain 20-45 wt% of the ZSM-5 zeolite, 10-35 wt% of a high stability matrix, 2-8 wt% of an alumina binder and 15-45 wt% of the clay.
[0035] The specific surface area of the catalytic cracking aid of the present invention can be 150 to 350 m 2 / g, the water droplet pore volume can be 0.25-0.45 mL / g, the wear index can be 0.5-3.5% / h, and the micro-reaction activity index can be 32-60.
[0036] The method of the catalytic cracking aid of the present invention comprises: mixing and slurrying water, clay, alumina binder, and a highly stable matrix to obtain a first slurry; after mixing the first slurry and the ZSM-5 zeolite, spray drying, roasting, and washing the obtained second slurry. The highly stable matrix of the present invention is prepared by the following steps: 1) slurrying the slag uniformly to a solid content of 10 to 20% by weight, and then grinding. 2) stirring the ground slag and the aluminum source uniformly
[0037] 3) adding concentrated phosphoric acid to control the total solid content to 25-45% by weight; 4) reacting the obtained slurry at 50-95°C for 60-150 minutes and then cooling to room temperature, wherein the pH value of the slurry is 0.5-3. Optionally, the solid content of the first slurry and the second slurry is 20-40% by weight.
[0038] Optionally, the aluminum source is one or a mixture of two or more of pseudo-boehmite, aluminum hydroxide, aluminum nitrate, aluminum chloride, and aluminum sol.
[0039] Optionally, the alumina binder is pseudo-boehmite, aluminum sol, or a mixture of both.
[0040] Optionally, the spray drying tower temperature is 120-200°C.
[0041] The calcination temperature is 260-550° C. Calcination is well known to those skilled in the art, and can be carried out in a muffle furnace or a tube furnace, for example, the calcination temperature can vary in a wide range, preferably 300-450° C., and the calcination time can be 1-5 hours. There is no specific limitation on the calcination atmosphere, which can be an air atmosphere or an inert atmosphere, and the inert atmosphere can contain an inert gas and / or nitrogen, and the inert gas includes helium, argon, etc.
[0042] The washing method comprises: performing exchange washing with one or more of dilute phosphoric acid, dilute hydrochloric acid, dilute sulfuric acid, dilute nitric acid and ammonium salt, the washing temperature is room temperature to 80°C, the washing time is 10 to 60 minutes, the pH is 0.5 to 6, the washing temperature is preferably 40 to 60°C, the washing time is preferably 20 to 30 minutes, and the washing pH is preferably 0.5 to 2
[0043] The method of the invention can realize the recycling of the rubber residue and can prepare a catalytic cracking aid with good cracking activity.
[0044] In a specific embodiment of the present invention, the method for preparing a catalytic cracking catalyst includes: mixing and slurrying water, clay, and an alumina binder to obtain a first slurry; mixing the first slurry and the ZSM-5 zeolite, and then slurrying a high-stability matrix to obtain a second slurry, and spray-drying, calcining, and washing the obtained second slurry.
[0045] The time for preparing the first slurry may be 30 to 120 minutes, and the time for preparing the second slurry may be 10 to 60 minutes. More preferably, the first slurry and ZSM-5 zeolite are mixed and stirred for 10 to 60 minutes, and then the high stability matrix is added and stirred for 10 to 30 minutes.
[0046] According to the present invention, ZSM-5 zeolite can be selected from HZSM-5 zeolite and / or modified ZSM-5 zeolite, and the modified ZSM-5 zeolite contains one or more of phosphorus, iron and rare earth metals; the rare earth metals can be Sc, Y, La, Ce, Pr, etc. Clay is well known to those skilled in the art and can be selected from one or more of kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite and sepiolite. The third aspect of the present invention provides an application of the catalytic cracking aid provided by the first aspect of the present invention in the catalytic cracking of crude oil.
[0047] According to the present invention, the conditions for catalytic cracking of crude oil may include: a temperature of 490-530° C. and a catalyst-to-oil ratio of 3-8.
[0048] According to the present invention, when the catalytic cracking aid of the present invention is used in a catalytic cracking process, it can be added to the catalytic cracking reactor alone or mixed with a catalytic cracking catalyst. In a specific embodiment, based on the total amount of the catalytic cracking aid and the cracking catalyst, the content of the catalytic cracking aid provided by the present invention is 1 to 50% by weight, preferably 5 to 30% by weight.
[0049] Example
[0050] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.
[0051] The slag is a discarded slag obtained by sedimentation, filtration and slag cutting of waste water generated in the production of catalytic cracking catalysts. The solid content of the slag is 20%. Based on the dry weight of the slag, it mainly contains 9.0 weight% of Na2O, 23.0 weight% of Al2O3, 48.0 weight% of SiO2 and 9.2 weight% of RE2O3.
[0052] Kaolin was produced by Suzhou Kaolin Company with a solid content of 76% by weight;
[0053] Pseudo-boehmite was produced by Shandong Aluminum Plant and had a solid content of 62.0 wt %;
[0054] Aluminum hydroxide was produced by Shandong Aluminum Plant with a solid content of 65.0 wt %;
[0055] Aluminum nitrate is produced by Beijing Chemical Plant, with analytical grade and content of 99.5%.
[0056] The aluminum sol has an aluminum oxide content of 21.5% by weight; it is produced by Sinopec Catalyst Co., Ltd.
[0057] Hydrochloric acid was produced by Beijing Chemical Plant with analytical grade and mass concentration of 36%;
[0058] Phosphoric acid was produced by Beijing Chemical Plant with analytical grade and mass concentration of 85%;
[0059] Nitric acid was produced by Beijing Chemical Plant with analytical grade and mass concentration of 68%;
[0060] Oxalic acid was produced by Beijing Chemical Plant and was analytically pure;
[0061] The solid content of HZSM-5 zeolite is 75 wt%, SiO2 / Al2O3=25, and the Na2O content is 0.15 wt%;
[0062] HZSM-5 zeolite is produced by Sinopec Catalyst Co., Ltd. and is analytically pure;
[0063] The ASAP 2405N V1.01 automatic adsorption instrument from Micromeritics of the United States was used, and the low-temperature static nitrogen adsorption capacity method was used. The sample was heated to 1.33×10 -2 The sample was vacuum degassed at 300 °C for 4 h, and the adsorption-desorption isotherm of the sample was measured at 77.4 K using N2 as the adsorption medium. The specific surface area (S BET ), measure the volume of N2 adsorbed by the sample when the relative pressure p / p0=0.98, and convert it into liquid nitrogen volume, i.e., pore volume;
[0064] The average pore size of the samples was determined using the Q / SH 3360-206 method;
[0065] The composition of the samples was determined by X-ray fluorescence spectroscopy (XRF);
[0066] The particle size of the sample was determined using the NB / SH / T 0951-2017 method;
[0067] NB / SH / T 0952-2017 was used to determine the micro-reaction index of catalytic cracking catalyst;
[0068] The apparent bulk density of catalytic cracking catalyst was determined using NB / SH / T 0954-2017;
[0069] The pore volume of catalytic cracking catalyst was determined using NB / SH / T 0955-2017;
[0070] NB / SH / T 0964-2017 was used to determine the wear index of catalytic cracking catalyst.
[0071] Example 1
[0072] S1. Preparation of high stability matrix: Add 543 g of slag into 291 g of water and stir evenly, grind with a ball mill, wherein the particle size is controlled to be D(V, 0.5) = 3.5 μm, D(V, 0.9) = 8.7 μm, add 58 g of pseudo-boehmite to the ground slag under high-speed stirring conditions, stir for 30 minutes, add 390 g of concentrated phosphoric acid at a uniform speed under stirring conditions, react at a constant temperature of 65 degrees (℃) for 90 minutes, and cool to 30℃ to form a high stability matrix GZ-1, whose pH value is 2.7.
[0073] S2. Preparation of catalytic cracking aid: 10 g of pseudo-boehmite, 42 g of aluminum sol, 90 g of kaolin and 174 g of decationized water are added to a pulping tank and pulped for 60 min, the pH is adjusted to 3.0, and then 385 g of the above-mentioned high stability matrix (GZ-1) and 300 g of HZSM-5 zeolite are added, stirred for 30 minutes, and then the obtained slurry is spray-dried to form, calcined at 500° C. for 2 hours, washed twice with ammonium sulfate exchange according to water: catalyst = 10:1 (weight ratio), and dried to obtain the catalytic cracking aid ZP-1 provided by the present invention. The characteristic parameters are shown in Table 1, and the same is true for the following embodiments.
[0074] Example 2
[0075] S1. Preparation of high-stability matrix: Add 545 g of slag into 373 g of water and stir evenly, grind with a ball mill, wherein the particle size is controlled to be D(V, 0.5) = 3.9 μm, D(V, 0.9) = 10.1 μm, add 135.5 g of pseudo-boehmite to the ground slag under high-speed stirring conditions, stir for 30 minutes, add 390 g of concentrated phosphoric acid at a uniform speed under stirring conditions, react at a constant temperature of 80 degrees for 90 minutes, and cool to 30°C to form a high-stability matrix GZ-2, and the pH value of the slurry is 3.4.
[0076] S2. Preparation of catalytic cracking aid: 14.5 g of pseudo-boehmite, 28 g of aluminum sol, 92 g of kaolin and 179 g of decationized water are added to a pulping tank and pulped for 60 minutes, the pH is adjusted to 2.8, and then 430 g of the above-mentioned high-stability matrix (GZ-2) and 257 g of HZSM-5 zeolite are added, and the mixture is homogenized and dispersed (stirred) for 30 minutes. The solid content of the obtained slurry is 30% by weight. The obtained slurry is then spray-dried and formed, calcined at 500° C. for 2 hours, washed twice with ammonium sulfate according to a ratio of water: catalyst = 10:1 and 3% by weight of the catalyst, and dried to obtain the catalytic cracking aid ZP-2 provided by the present invention.
[0077] Example 3
[0078] S1. Preparation of high stability matrix: 392 g of slag was added to 300 g of water and stirred evenly, and ground by ball mill, wherein the particle size was controlled to be D(V, 0.5) = 2.1 μm, D(V, 0.9) = 5.3 μm, and 50 g of 20% nitric acid solution was added under stirring to adjust the pH to 3, and the mixture was reacted at 80°C for 60 minutes under stirring. After the mixture was cooled to 30°C, 18 g of pseudo-boehmite was added to the ground slag under high-speed stirring and stirred for 30 minutes. Under stirring, 390 g of concentrated phosphoric acid was added at a uniform speed, and the mixture was reacted at 90°C for 120 minutes. The mixture was cooled to 30°C to form a high stability matrix GZ-3, and the pH value of the slurry was 0.8.
[0079] S2. Preparation of catalytic cracking aid: 48 g of pseudo-boehmite, 28 g of aluminum sol, 146 g of kaolin and 265 g of decationized water are added to a pulping tank and pulped for 60 minutes, the pH is adjusted to 2.1, and then 347 g of the above-mentioned high-stability matrix (GZ-2) and 171 g of HZSM-5 zeolite are added, and the mixture is homogenized and dispersed (stirred) for 30 minutes. The obtained slurry is then spray-dried and formed, calcined at 500° C. for 2 hours, washed twice with ammonium sulfate according to a ratio of water: catalyst = 10:1 and 3% by weight of the catalyst, and dried to obtain the catalytic cracking aid ZP-3 provided by the present invention.
[0080] Example 4
[0081] S1. Preparation of high-stability matrix: Add 303 g of slag into 104 g of water and stir evenly, grind with a ball mill, wherein the particle size is controlled to be D(V, 0.5) = 3.1 μm, D(V, 0.9) = 8.3 μm, add 32 g of pseudo-boehmite to the ground slag under high-speed stirring conditions, stir for 30 minutes, add 162 g of concentrated phosphoric acid at a uniform speed under stirring conditions, react at a constant temperature of 80 degrees for 90 minutes, and cool to 30°C to form a high-stability matrix GZ-4, and the pH value of the slurry is 3.1.
[0082] S2. Preparation of catalytic cracking aid: 69 g of aluminum sol, 200 g of kaolin and 304 g of decationized water are added to a pulping tank and pulped for 60 minutes, then 170 g of the above-mentioned high-stability matrix (GZ-4) and 257 g of HZSM-5 zeolite are added, and the mixture is homogenized and dispersed (stirred) for 30 minutes, and then the obtained slurry is spray-dried and formed, calcined at 500° C. for 2 hours, washed twice with ammonium sulfate according to a ratio of water: catalyst = 10:1 and 3% by weight of the catalyst, and dried to obtain the catalytic cracking aid ZP-4 provided by the present invention.
[0083] Example 5
[0084] S1. Preparation of high-stability matrix: Add 506 g of slag into 130 g of water and stir evenly, grind with a ball mill, wherein the particle size is controlled to be D(V, 0.5) = 3.5 μm, D(V, 0.9) = 8.7 μm, add 22 g of aluminum hydroxide to the ground slag under high-speed stirring conditions, stir for 30 minutes, add 260 g of concentrated phosphoric acid at a uniform speed under stirring conditions, react at a constant temperature of 75 degrees for 90 minutes, and cool to 30°C to form a high-stability matrix GZ-5, and the pH value of the slurry is 2.9.
[0085] S2. Preparation of catalytic cracking aid: 69 g of aluminum sol, 114 g of kaolin and 198 g of decationized water are added to a pulping tank and pulped for 60 minutes, then 275 g of the above-mentioned high-stability matrix (GZ-5) and 343 g of HZSM-5 zeolite are added, and the mixture is homogenized and dispersed (stirred) for 30 minutes, and then the obtained slurry is spray-dried and formed, calcined at 500° C. for 2 hours, washed twice with ammonium sulfate according to a ratio of water: catalyst = 10:1 and 3% by weight of the catalyst, and dried to obtain the catalytic cracking aid ZP-5 provided by the present invention.
[0086] Example 6
[0087] S1. Preparation of high-stability matrix: Add 506 g of slag to 521 g of water and stir evenly, grind with a ball mill, wherein the particle size is controlled to be D(V, 0.5) = 3.7 μm, D(V, 0.9) = 8.9 μm, add 93.6 g (aluminum nitrate concentration 67.5%) of aluminum nitrate solution to the ground slag under high-speed stirring conditions, stir for 30 minutes, add 260 g of concentrated phosphoric acid at a uniform speed under stirring conditions, react at a constant temperature of 75 degrees for 90 minutes, and then cool to 30°C to form a high-stability matrix GZ-6, and the pH value of the slurry is 2.6.
[0088] S2. Preparation of catalytic cracking aid: 55 g of aluminum sol, 114 g of kaolin and 226 g of decationized water are added to a pulping tank and pulped for 60 minutes, the pH is adjusted to 2.0, and then 275 g of the above-mentioned high-stability matrix (GZ-6) and 300 g of HZSM-5 zeolite are added, and the mixture is homogenized and dispersed (stirred) for 30 minutes. The obtained slurry is then spray-dried and formed, calcined at 500° C. for 2 hours, washed twice with ammonium sulfate according to a ratio of water: catalyst = 10:1 and 3% by weight of the catalyst, and dried to obtain the catalytic cracking aid ZP-6 provided by the present invention.
[0089] Example 7
[0090] S1. Preparation of high stability matrix: 181 g of slag was added to 180 g of water and stirred evenly, and ground by ball mill, wherein the particle size was controlled to be D(V, 0.5) = 1.5 μm, D(V, 0.9) = 3.7 μm, 45 g of pseudo-boehmite and 216 g of water were added to the ground slag under high-speed stirring conditions, and stirred for 30 minutes. Under stirring conditions, 389 g of concentrated phosphoric acid was added at a uniform speed, and the reaction was carried out at a constant temperature of 75 degrees for 90 minutes, and then cooled to 30 degrees to form a high stability matrix GZ-7, and the pH value of the slurry was 0.9.
[0091] S2. Preparation of catalytic cracking aid: 42 g of aluminum sol, 195 g of kaolin and 312 g of decationized water are added to a pulping tank and pulped for 60 min, then 150 g of the above-mentioned high-stability matrix (GZ-5) and 300 g of HZSM-5 zeolite are added, and the mixture is homogenized and dispersed (stirred) for 30 minutes, and then the obtained slurry is spray-dried and formed, calcined at 500° C. for 2 hours, washed twice with ammonium sulfate according to a ratio of water: catalyst = 10:1 and 3% by weight of the catalyst, and dried to obtain the catalytic cracking aid ZP-7 provided by the present invention.
[0092] Example 8
[0093] S1. Preparation of high stability matrix: 72g of slag was added to 70g of water and stirred evenly, and ground by ball mill, wherein the particle size was controlled to be D(V, 0.5) = 1.9μm, D(V, 0.9) = 4.2μm, and 100g of 10% oxalic acid solution was added under stirring to adjust the pH to 4, and the mixture was reacted at 80°C for 60 minutes under stirring. After the mixture was cooled to 30°C, 370g of water and 147g of aluminum hydroxide were added to the ground slag under high-speed stirring, and stirred for 30 minutes. Under stirring, 389g of concentrated phosphoric acid was added at a uniform speed, and the mixture was reacted at 75°C for 90 minutes. The mixture was cooled to 30°C to form a high stability matrix GZ-8, and the pH value of the slurry was 3.3.
[0094] S2. Preparation of catalytic cracking aid: 69 g of aluminum sol, 94 g of kaolin and 176 g of decationized water are added to a pulping tank and pulped for 60 minutes, then 302 g of the above-mentioned high-stability matrix (GZ-5) and 385 g of HZSM-5 zeolite are added, and the mixture is homogenized and dispersed (stirred) for 30 minutes, and then the obtained slurry is spray-dried and formed, calcined at 500° C. for 2 hours, washed twice with ammonium sulfate according to a ratio of water: catalyst = 10:1 and 3% by weight of the catalyst, and dried to obtain the catalytic cracking aid ZP-8 provided by the present invention.
[0095] Example 9
[0096] S1. Preparation of high stability matrix: 1636 g of slag was added to 850 g of water and stirred evenly. The slag was ground using a ball mill, wherein the particle size was controlled to be D(V, 0.5) = 1.1 μm, D(V, 0.9) = 2.8 μm. 19 g of pseudo-boehmite was added to the ground slag under high-speed stirring conditions and stirred for 30 minutes. 389 g of concentrated phosphoric acid was added at a uniform rate under stirring conditions. The reaction was carried out at a constant temperature of 75 degrees for 90 minutes, and then cooled to 30 degrees to form a high stability matrix GZ-9. The pH value of the slurry was 3.4.
[0097] S2. Preparation of catalytic cracking aid: 96 g of aluminum sol, 179 g of kaolin, 24 g of pseudo-boehmite and 285 g of decationized water are added to a pulping tank and pulped for 60 minutes, the pH is adjusted to 3.0, and then 300 g of the above-mentioned high-stability matrix (GZ-5) and 214 g of HZSM-5 zeolite are added, and the mixture is homogenized and dispersed (stirred) for 30 minutes. The obtained slurry is then spray-dried and formed, calcined at 500° C. for 2 hours, washed twice with ammonium sulfate according to a ratio of water: catalyst = 10:1 and 3% by weight of the catalyst, and dried to obtain the catalytic cracking aid ZP-9 provided by the present invention.
[0098] Comparative Example 1
[0099] This comparative example illustrates the cracking aid prepared by using conventional phosphorus-modified aluminum sol and unmodified slag.
[0100] The phosphorus-aluminum matrix PA-D was prepared according to the method of Example 1 in CN1417296A. The specific method is as follows:
[0101] 371 g of pseudo-boehmite and 879 g of decationized water were slurried for 30 minutes, 1250 g of concentrated phosphoric acid was added to the slurry under stirring, the temperature was raised to 70°C, and then reacted at this temperature for 45 minutes to obtain a colorless and transparent phosphorus-containing aluminum sol.
[0102] According to the method of Example 1 of the present invention, 42g of aluminum sol, 89g of kaolin, 160g of slag, and 119g of decationized water were added to a pulping tank and pulped for 60min, the pH was adjusted to 3.0, and then 300g of HZSM-5 zeolite was added, stirred for 30min, and finally 210g of the above-mentioned matrix (PA-D) was added and stirred for 30 minutes. The obtained slurry had a solid content of 30%, and then the obtained slurry was spray-dried and formed, calcined at 500°C for 2 hours, washed twice with ammonium sulfate according to water: catalyst = 10:1, 3% by weight of the catalyst, and dried to obtain a comparative catalytic cracking aid ZP-D1, whose characteristic parameters are shown in Table 2, and the same is true for the following comparative examples.
[0103] Comparative Example 2
[0104] This comparative example illustrates the use of conventional phosphorus-modified aluminum sol and a cracking aid prepared without slag.
[0105] The phosphorus-modified aluminum sol PA-D was prepared in the same manner as in Comparative Example 1.
[0106] According to the method of Example 1 of the present invention, 42g of aluminum sol, 133g of kaolin and 235g of decationized water were added to a slurrying tank and slurried for 60min. The pH was adjusted to 3.0 and then 300g of HZSM-5 zeolite was added and stirred for 30min. Finally, 210g of the above-mentioned matrix (PA-D) was added and homogenized (stirred) for 30 minutes. The obtained slurry had a solid content of 30%. The obtained slurry was spray dried and formed, calcined at 500°C for 2 hours, washed twice with ammonium sulfate according to water: catalyst = 10:1 and 3% by weight of the catalyst, and dried to obtain a comparative catalytic cracking aid ZP-D2.
[0107] Table 1 Composition and physicochemical properties of catalytic cracking additives
[0108]
[0109]
[0110] Table 2 Composition and physicochemical properties of catalytic cracking additives
[0111]
[0112] Test Case
[0113] The catalytic cracking aids ZP1 to ZP9 prepared in Examples 1 to 9 of the present invention, the catalytic cracking aids ZP-D1 to ZP-D2 prepared in Comparative Examples 1 to 2 and the industrial catalyst of grade CMT-1 (provided by Sinopec Catalyst Qilu Branch, main properties are shown in Table 3) were mixed into a catalyst mixture according to the proportion, and the catalyst mixture was aged at 800°C and 100% water vapor for 17 hours in a fixed bed aging device. Then, the catalyst mixture was evaluated on the ACE device, and the properties of the raw oil used for evaluation are shown in Table 4. The reaction temperature, catalyst-oil ratio, weight hourly space velocity and evaluation results are listed in Table 5.
[0114] Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield;
[0115] Propylene concentration in liquefied gas = propylene yield / liquefied gas yield.
[0116] Table 3 Properties of industrial catalysts
[0117]
[0118]
[0119] Table 4 Raw oil properties
[0120] project data <![CDATA[Density (20 °C) / (kg·cm -3 )]]> 922.8 w(residual carbon value) / % 3.62 w(C) / % 86.77 w(H) / % 12.08 w(S) / % 0.6 w(N) / % 0.26 <![CDATA[Mass fraction of metal / (μg·g -1 )]]> Fe 4.6 Ni 10.4 V 4.7 Mass fraction of four components / % Saturated hydrocarbons 58.8 Aromatics 26.4 Gel 14 Asphaltene 0.8
[0121] Table 5 Evaluation results
[0122]
[0123]
[0124]
[0125] Table 6 Evaluation results
[0126]
[0127] It can be seen from Table 5 and Table 6 that the catalytic cracking aid prepared by the method of the present invention has an excellent propylene yield, can significantly increase the concentration of propylene in liquefied gas, and has high cracking activity.
[0128] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0129] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0130] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A catalytic cracking aid, It is characterized in that Based on the total weight of the catalytic cracking aid, the catalytic cracking aid contains: (1) 15 to 55 weight percent of a zeolite having an MFI structure; (2) 2 to 20 weight percent of an alumina binder; (3) 10 to 50 weight percent of a highly stable matrix, which contains 0.1 to 10.0 weight percent of Na 2 O, 5 to 35 wt% Al 2 O 3 , 5~25 wt% SiO 2 , 30~80 wt% P 2 O 5 , 1~10 wt% RE 2 O 3 ; (4) 10 to 50 weight percent clay; The highly stable matrix is prepared by the following steps: 1) beating the slurry evenly to a solid content of 10-20% by weight, and then grinding; 2) adding acid to the ground slurry, adjusting the pH to 2-5, heating to 70-150° C. for constant temperature reaction for 30-150 minutes, and then cooling to 10-50° C.; 3) stirring the ground slurry or the slurry obtained in step 2) evenly with an aluminum source; 4) adding concentrated phosphoric acid to control the total solid content of the slurry to be 25-45% by weight; 4) reacting the obtained slurry at 50-95° C. for 60-150 minutes and then cooling to 10-50° C.; the pH value of the obtained slurry is 0.5-3.5, i.e., a highly stable matrix; wherein the weight ratio of the slurry to the aluminum source is 0.1-30:1, and the weight of the aluminum source is calculated as alumina; the above step 2) is an optional step.
2. A method for preparing the catalytic cracking aid according to claim 1, the method comprising preparing a highly stable matrix; the highly stable matrix is prepared by the following steps: 1) slurrying the slurry uniformly, with a solid content of 10-20% by weight, and grinding; 2) adding acid to the ground slurry, adjusting the pH to 2-5, heating to 70-150°C for constant temperature reaction for 30-150 minutes, and then cooling to 10-50°C; 3) stirring the ground slurry or the slurry obtained in step 2) with an aluminum source uniformly; 4) adding concentrated phosphoric acid to control the total solid content of the slurry to be 25-45% by weight; 4) reacting the obtained slurry at 50-95°C for 60-150 minutes and then cooling to 10-50°C; the pH value of the obtained slurry is 0.5-3.5, i.e., a highly stable matrix; wherein the weight ratio of the slurry to the aluminum source is 0.1-30:1, and the weight of the aluminum source is calculated as alumina; the above step 2) is an optional step.
3. The method according to claim 2, wherein the slag contains 10 to 50% by weight of Al 2 O 3 , 30~70 wt% SiO 2 , 2~15 wt% Na 2 O and 1-15 wt% RE 2 O 3 .
4. The method according to claim 2, in, The particle size of the slag is controlled to be D(V,0.5)≤5μm, D(V,0.9)≤15μm.
5. The method according to any one of claims 2 to 4, in, The aluminum source is selected from one or more of pseudo-boehmite, aluminum hydroxide, aluminum sol, aluminum nitrate, aluminum chloride, and aluminum sulfate.
6. The method according to claim 2, in, The method further comprises the steps of mixing water, zeolite with MFI structure, high stability matrix, alumina binder and clay and then spray drying, calcining and washing.
7. The method according to claim 6, in, The method comprises: (1) mixing water, clay and alumina binder to obtain a first slurry; (2) mixing and beating the first slurry, the zeolite having an MFI structure and the high-stability matrix to obtain a second slurry; and (3) The obtained second slurry is spray-dried, calcined and washed.
8. The method according to claim 7, wherein the solid content of the first slurry and the second slurry is 20-40 wt%.
9. The method according to claim 2, wherein the alumina binder is selected from one or both of pseudo-boehmite and alumina sol.
10. The method according to claim 2, in, The zeolite with MFI structure is selected from ZSM-5 zeolite; the clay is selected from one or more of kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite and sepiolite.
11. Use of the catalytic cracking aid according to claim 1 in catalytic cracking of crude oil.