A device for preventing tundish water outlet from being blocked and a manufacturing method thereof

By using solid semicircular rings and hollow cylindrical structures made of materials such as scale graphite, combined with ultrasonic probes and refractory coatings, the problem of blockage of metallurgical continuous casting tundra water outlet is solved. Improves the efficiency and product quality of the continuous casting process.

CN116100011BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310024847.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-09
Publication Date
2024-12-03
Estimated Expiration
2043-01-09

AI Technical Summary

Technical Problem

The problem of blockage in the tung-intermediate water outlet during metallurgical continuous casting leads to liquid level fluctuations, affecting product quality, reducing metal yield and limiting production efficiency. The manufacturing process of the existing technology is complex and the air permeable material is prone to cracks and low argon blowing efficiency.

Method used

Using solid semicircular rings and hollow cylindrical structures made of flake graphite, magnesium phosphate, magnesium oxide and other materials, combined with ultrasonic probes and refractory coatings, anti-blocking devices are created through pressurized sintering process, and ultrasonic mechanical effects and air The chemical action prevents the water outlet from being blocked.

Benefits of technology

It achieves efficient prevention of water outlet blockage, improves the density and durability of the device, and does not need to be replaced for a long time, improves the purity of the steel and the continuous casting furnace, avoiding the leakage and inefficiency problems of traditional argon blowing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116100011B_ABST
    Figure CN116100011B_ABST
Patent Text Reader

Abstract

The present invention relates to a device for preventing the tundish water inlet from being blocked and a manufacturing method thereof, comprising a solid semicircular ring structure, a hollow cylindrical structure, an ultrasonic probe, a horn, and a transducer. The hollow cylindrical structure is integrally connected to the solid semicircular ring structure, the inner arc of the solid semicircular ring structure matches the outer arc of the water inlet, the ultrasonic probe, the horn, and the transducer are sequentially connected inside the hollow structure, the transducer is connected to the ultrasonic generator through a wire, and the surface of the ultrasonic probe is covered with a refractory coating. The hollow and solid structures of the device of the present invention have high density and good durability, and can be used for a long time without replacement. The present invention is installed on the water inlet, and uses the ultrasonic mechanical effect to prevent the water inlet from being blocked, and the method of use is simple. A high-density water inlet can be selected in combination, and no air gap is required. The present invention can use the cavitation effect of ultrasound to promote the floating of inclusions near the upper water inlet of the tundish, reduce the size of the inclusions, and thus improve the purity of the molten steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgical continuous casting, and in particular relates to a device for preventing a tundish water outlet from being blocked and a manufacturing method thereof. Background Art

[0002] During the continuous casting process, the blockage of the tundish nozzle is a major problem that troubles metallurgical workers. First, nozzle nodules or blockages will cause liquid level fluctuations, which will indirectly or directly affect the quality of the final product; secondly, nozzle blockage will also reduce the metal recovery rate, which is not conducive to cost control; more importantly, nozzle nodules or blockages will limit the number of continuous casting furnaces, affecting the normal production rhythm between steelmaking and continuous casting, and thus affecting the efficiency of large-scale production.

[0003] As a key component connecting the tundish and the crystallizer during the continuous casting process, the tundish nozzle plays an important role. It consists of an upper nozzle and an immersion nozzle. The upper nozzle is installed at the bottom of the tundish and controls the flow of molten steel by moving up and down with the integral stopper rod; the immersion nozzle is connected to the upper nozzle. During the continuous casting process, the molten steel in the ladle flows through the tundish, passes through the upper nozzle and the immersion nozzle in turn, and finally reaches the crystallizer. The nozzle blockage mechanism is as follows: (1) When the molten steel passes through the inner wall of the nozzle, it will react with the refractory material, which will cause the smoothness of the nozzle surface to decrease, providing favorable conditions for the later nozzle "nodulation". (2) High-melting-point inclusions formed by deoxidation during smelting and refining enter the nozzle channel during the pouring process and "nodulate". For example, when producing aluminum-killed steel or high-aluminum steel, the reaction between aluminum and oxygen in steel will inevitably produce alumina inclusions, which are solid at the continuous casting temperature and are easily accumulated at the tundish nozzle to cause blockage. In addition, cold steel blockage is easy to cause when the pouring temperature is low.

[0004] At present, various steel mills and scientific research institutions have conducted a lot of research mainly on promoting the effective removal of inclusions and inclusion modification, such as:

[0005] Chinese patent document CN102416451B discloses an anti-clogging tundish water inlet and its manufacturing method. The anti-clogging tundish water inlet is composed of three parts: the bowl and the inner layer are made of anti-clogging zirconium calcium carbon material; the outer layer and the bottom are made of aluminum zirconium carbon materials with different components. During use, it is not necessary to blow argon gas, which can effectively prevent the inner wall of the water inlet from being blocked. It uses the CaO decomposed by calcium zirconate in the inner layer material at the use temperature to react with Al2O3 in the molten steel to form a low melting point phase. Its design principle is to modify the inclusions.

[0006] Chinese patent document CN107321945A provides a method for removing inclusions by blowing argon through the air-permeable upper nozzle seat bricks of a continuous casting tundish. In each furnace, a proper amount of high-basicity, low-carbon tundish covering agent is added to the molten steel surface in the area just above the air-permeable upper nozzle seat bricks of the continuous casting tundish. This method can not only alleviate the problem of large fluctuations in the molten steel surface caused by blowing argon through the air-permeable upper nozzle seat bricks of the continuous casting tundish, but also more effectively prevent the secondary oxidation of the molten steel and slag rolling problems, thereby improving the metallurgical effect of removing inclusions by blowing argon through the air-permeable upper nozzle seat bricks of the continuous casting tundish. The design principle is to improve the efficiency of removing inclusions.

[0007] Chinese patent document CN213257089U discloses a multifunctional continuous casting tundish upper nozzle, the pouring hole of the tundish upper nozzle (from top to bottom includes three sections, namely section A, section B and section C, wherein section A is a cone with a large top and a small bottom, section B is a cone with a small top and a large bottom, section C is cylindrical, an arc transition is adopted between section A and section B, and the inner wall of section B is stepped from top to bottom; the upper part of section C is embedded with a refractory material with good air permeability, and a steel wire mesh is provided on the outer surface of the refractory material with poor air permeability corresponding to section C; a circle of argon flow grooves is provided around the pouring hole at the bottom of the tundish upper nozzle. It can slow down the deviation of steel flow and the blockage of nozzle. The shapes of sections A, B and C of the nozzle described in the patent are different, the processing and connection are complicated, and the connection strength is difficult to guarantee.

[0008] The traditional tundish nozzle is mostly made of aluminum zirconium carbon and uses argon blowing technology to avoid nozzle blockage. The nozzle needs to be made of permeable material and set with an air gap. Its technical defects are: 1) The manufacturing process is complicated; 2) The nozzle has a high porosity and relatively low strength. The permeable material is prone to cracks, and the molten steel is prone to flow out through the argon blowing channel along the air gap, causing accidents. 3) The argon blowing pipeline and the nozzle interface are prone to leakage. The porous material of the nozzle will also lead to low argon blowing efficiency and insufficient effective argon blowing flow. Summary of the invention

[0009] The present invention provides a device for preventing the clogging of the water inlet of the tundish and a manufacturing method thereof. Two sets of anti-clogging devices are installed on the outer wall of the water inlet of the tundish. An ultrasonic generating device with a coating is arranged in the device. The mechanical effect and cavitation effect of ultrasonic waves are used to prevent the clogging of the water inlet. The device body is prepared by a unique raw material ratio and a pressure sintering process, which improves the durability of the device body and the internal ultrasonic device. No replacement is required for a long time, which can help prevent the clogging of the water inlet during efficient continuous casting.

[0010] In order to achieve the above object, the present invention adopts the following technical solutions:

[0011] A device for preventing clogging of a tundish water nozzle comprises a solid semicircular ring structure, a hollow cylindrical structure, an ultrasonic probe, a horn, and a transducer. The hollow cylindrical structure is integrally connected to the solid semicircular ring structure, the inner arc of the solid semicircular ring structure matches the outer arc of the water nozzle, the ultrasonic probe, the horn, and the transducer are sequentially connected inside the hollow cylindrical structure, the transducer is connected to an ultrasonic generator via a wire, and the surface of the ultrasonic probe is covered with a refractory coating.

[0012] The two groups of devices for preventing the tundish water outlet from being blocked are mounted on the outer side of the water outlet in a buckled manner.

[0013] The solid semicircular ring structure and the hollow cylindrical structure are prepared from the following raw materials in parts by weight: 30-35 parts of flake graphite, 20-30 parts of dolomite powder, 5-10 parts of silicon dioxide, 15-20 parts of magnesium oxide, 5-15 parts of additives, and 8-10 parts of epoxy resin.

[0014] The additive is one or a combination of clay, quartz sand and dolomite.

[0015] The refractory coating is prepared from the following raw materials in parts by weight: 20-40 parts of aluminum oxide, 30-45 parts of calcium oxide, 30-35 parts of silica sol, and 0-3 parts of bentonite.

[0016] The method for preparing the refractory coating is as follows: the raw materials of the refractory coating are mixed evenly, then applied on the surface of the ultrasonic probe, and dried at a temperature of 520°C to 600°C for 1h to 2h.

[0017] A method for manufacturing a device for preventing tundish water inlet from being blocked, wherein the solid semicircular ring structure and the hollow cylindrical structure of the device are formed by an integrated molding method, and the specific method comprises:

[0018] 1) Put flake graphite, magnesite powder, silicon dioxide, magnesium oxide and additives into a container and place it on a vibration table for vibration;

[0019] 2) Add epoxy resin into the container, turn on the vibration switch, and make it vibrate up and down and horizontally in sequence. The up and down vibration time is 10 to 30 minutes, and the horizontal vibration time is 10 to 30 minutes;

[0020] 3) Add the raw materials in the container into the mold and form it in a pressure sintering machine. As the temperature rises, the sintering pressure is continuously increased. The final forming temperature is 950-1300° C. and the final forming pressure is 150MPa-180MPa.

[0021] 4) The integrally formed solid semicircular ring structure and hollow cylindrical structure are cooled for 1 to 2 hours before fine processing, and the ultrasonic probe, horn and transducer coated with a refractory coating are placed into the hollow cylindrical structure, and the transducer is connected to the ultrasonic generator through a wire.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1) The hollow and solid structures of the device manufactured by the present invention have high density and good durability, and can be used for a long time without replacement.

[0024] 2) The present invention is installed on the nozzle, and the power and frequency of the ultrasonic generator are adjusted according to the type of steel being smelted and the process, and the ultrasonic mechanical effect is used to prevent the nozzle from being blocked. The method of use is simple. A high-density nozzle can be selected in combination, and no air gap is required.

[0025] 3) The present invention can utilize the cavitation effect of ultrasound to promote the floating of inclusions near the upper water inlet of the tundish, reduce the size of the inclusions, and thus improve the purity of the molten steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic structural diagram of the anti-blocking device of the present invention;

[0027] Figure 2 is a front cross-sectional view of the device of the present invention applied to a nozzle;

[0028] Figure 3 It is a top cross-sectional view of the device of the present invention applied to a water outlet.

[0029] In the figure: 1. Device for preventing tundish water inlet from being blocked; 2. Solid semicircular ring structure; 3. Hollow cylindrical structure; 4. Ultrasonic probe; 5. Refractory coating; 6. Amplitude transformer; 7. Transducer; 8. Conductor; 9. Ultrasonic generator; 10. Water inlet. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0031] See Figure 1-Figure 3 A device for preventing clogging of a tundish nozzle comprises a solid semicircular ring knot 2, a hollow cylindrical structure 3, an ultrasonic probe 4, a horn 6, and a transducer 7. The hollow cylindrical structure 3 is integrally connected to the solid semicircular ring structure 2. The inner arc of the solid semicircular ring structure 2 matches the outer arc of the nozzle. The ultrasonic probe 4, the horn 6, and the transducer 7 are sequentially connected inside the hollow cylindrical structure. The transducer 7 is connected to an ultrasonic generator 9 via a wire 8. The surface of the ultrasonic probe 4 is covered with a refractory coating 5.

[0032] The two groups of devices 1 for preventing clogging of the tundish water inlet are mounted on the outer side of the water inlet 10 in a buckled manner.

[0033] The solid semicircular ring structure 2 and the hollow cylindrical structure 3 are prepared from the following raw materials in parts by weight: 30-35 parts of flake graphite, 20-30 parts of dolomite powder, 5-10 parts of silicon dioxide, 15-20 parts of magnesium oxide, 5-15 parts of additives, and 8-10 parts of epoxy resin.

[0034] The additive is one or a combination of clay, quartz sand and dolomite.

[0035] The refractory coating 5 is prepared from the following raw materials in parts by weight: 20-40 parts of aluminum oxide, 30-45 parts of calcium oxide, 30-35 parts of silica sol, and 0-3 parts of bentonite.

[0036] The manufacturing method of the refractory coating 5 is as follows: the raw materials of the refractory coating are mixed evenly and then applied on the surface of the ultrasonic probe 4, and then dried at a temperature of 520° C. to 600° C. for 1 h to 2 h.

[0037] A method for manufacturing a device for preventing tundish water inlet from being blocked, wherein the solid semicircular ring structure 2 and the hollow cylindrical structure 3 of the device are formed by an integrated molding method, and the specific method includes:

[0038] 1) Put flake graphite, magnesite powder, silicon dioxide, magnesium oxide and additives into a container and place it on a vibration table for vibration;

[0039] 2) Add epoxy resin into the container, turn on the vibration switch, and make it vibrate up and down and horizontally in sequence. The up and down vibration time is 10 to 30 minutes, and the horizontal vibration time is 10 to 30 minutes;

[0040] 3) Add the raw materials in the container into the mold and form it in a pressure sintering machine. As the temperature rises, the sintering pressure is continuously increased. The final forming temperature is 950-1300° C. and the final forming pressure is 150MPa-180MPa.

[0041] 4) The integrally formed solid semicircular ring structure 2 and hollow cylindrical structure 3 are cooled for 1 to 2 hours before fine processing, and the ultrasonic probe 4, horn 6, and transducer 7 coated with a refractory coating are placed into the hollow cylindrical structure 3, and the transducer 7 is connected to the ultrasonic generator 9 via a wire 8.

[0042] Embodiment 1:

[0043] The solid semicircular ring structure 2 and the hollow cylindrical structure 3 are mixed according to the following weight ratio:

[0044] 35 parts of flake graphite, 25 parts of magnesite powder, 8 parts of silicon dioxide, 18 parts of magnesium oxide, 14 parts of additives and 9 parts of epoxy resin;

[0045] The additive consists of clay and quartz sand, wherein the weight ratio of clay is 70% of the total weight of the additive; the weight ratio of quartz sand is 30% of the total weight of the additive, and the particle size is 0.1 mm < 0.5 mm.

[0046] The refractory coating 5 is prepared according to the following proportions:

[0047] 22 parts of aluminum oxide, 43 parts of calcium oxide, 32 parts of silica sol, and 3 parts of bentonite; mix them evenly and apply them on the surface of the ultrasonic probe 4, and dry them at 540°C for 1 hour.

[0048] The solid semicircular ring structure 2 and the hollow cylindrical structure 3 of the device for preventing the tundish upper water inlet from being blocked are manufactured by an integrated molding method according to the following process:

[0049] 1) 35 parts of flake graphite, 25 parts of magnesite powder, 8 parts of silicon dioxide, 18 parts of magnesium oxide, and 14 parts of additives are placed in a container and vibrated up and down and left and right.

[0050] 2) Place the container on a vibration table, add epoxy resin, and turn on the vibration switch to vibrate it up and down and horizontally in turn. The up and down vibration time is 10 minutes, and the horizontal vibration time is 30 minutes.

[0051] 3) Add the raw materials in the container into the mold and form it in a pressure sintering machine. The sintering pressure is continuously increased as the temperature rises. The final forming temperature is 960° C. and the final forming pressure is 175 MPa.

[0052] 4) The formed device is cooled for 1 hour before fine processing, and the coated ultrasonic probe 4, horn 6, and transducer 7 are placed into the hollow cylindrical structure 3, and the transducer 7 is connected to the ultrasonic generator 9 through a wire 8.

[0053] After testing, the physical performance indicators of the main structure of the solid semicircular structure 2 and the hollow cylindrical structure 3 of the device for preventing the tundish upper water inlet from being blocked are: volume density 4.5g / cm 3 ; Raw material true density 4.7g / cm 3 ; Calculated relative density (bulk density / true density) = 95.7%; refractoriness 1839℃; room temperature flexural strength 24.6Mpa. This shows that the device has excellent density and thermal stability

[0054] During the continuous casting process of aluminum-killed steel, the device was applied to the tundish water inlet. The device had good thermal stability, the coating on the probe surface did not fall off and there was no corrosion. The number of continuous pouring furnaces was increased to 22, and the number of continuous pouring furnaces was greatly increased.

[0055] Embodiment 2:

[0056] The solid semicircular structure 2 and the hollow cylindrical structure 3 are mixed according to the following weight ratio:

[0057] 32 parts of flake graphite, 30 parts of magnesite powder, 10 parts of silicon dioxide, 20 parts of magnesium oxide, 8 parts of additives and 8 parts of epoxy resin;

[0058] The additive consists of clay and quartz sand, wherein the weight ratio of clay is 60% of the total weight of the additive; the weight ratio of quartz sand is 40% of the total weight of the additive, and the particle size is 0.1 mm < 0.5 mm.

[0059] The refractory coating 5 is prepared according to the following proportions:

[0060] 36 parts of aluminum oxide, 32 parts of calcium oxide, 30 parts of silica sol, and 2 parts of bentonite; mix them evenly, apply them on the surface of the ultrasonic probe, and dry them at 600°C for 1.5 hours.

[0061] The solid semicircular ring structure 2 and the hollow cylindrical structure 3 of the device for preventing the tundish upper water inlet from being blocked are manufactured by an integrated molding method according to the following process:

[0062] 1) Place 32 parts of flake graphite, 30 parts of magnesite powder, 10 parts of silicon dioxide, 20 parts of magnesium oxide, and 8 parts of additives in a container and vibrate it up and down and left and right.

[0063] 2) Place the container on a vibration table, add epoxy resin, and turn on the vibration switch to vibrate it up and down and horizontally in sequence. The up and down vibration time is 15 minutes, and the horizontal vibration time is 15 minutes.

[0064] 3) Add the raw materials in the container into the mold and form it in a pressure sintering machine. The sintering pressure is continuously increased as the temperature rises. The final forming temperature is 1270° C. and the final forming pressure is 170 MPa.

[0065] 4) After the main structure is formed, it is cooled for 1.5 hours before fine processing. The coated ultrasonic probe 4, horn 6, and transducer 7 are placed into the hollow cylindrical structure 3, and the transducer 7 is connected to the ultrasonic generator 9 through a wire 8.

[0066] After testing, the physical performance indicators of the solid semicircular structure 2 and the hollow cylindrical structure 3 of the device for preventing the tundish upper water inlet from being blocked are: volume density 4.4g / cm 3 ; Raw material true density 4.6g / cm 3 ; Calculated relative density (bulk density / true density) = 95.6%; refractoriness 1749℃; room temperature flexural strength 23.2Mpa. This shows that the device has excellent density and thermal stability

[0067] During the continuous casting of aluminum-killed steel, the device was applied to the tundish nozzle. The device had good thermal stability, and the probe surface coating did not fall off or corrode. The number of continuous casting furnaces increased to 23, and the number of continuous casting furnaces increased significantly.

[0068] Embodiment 3:

[0069] The solid semicircular structure 2 and the hollow cylindrical structure 3 are mixed according to the following weight ratio:

[0070] 30 parts of flake graphite, 28 parts of magnesite powder, 9 parts of silicon dioxide, 15 parts of magnesium oxide, 18 parts of additives and 10 parts of epoxy resin;

[0071] The additive is composed of clay, quartz sand and dolomite, wherein the weight ratio of clay is 50% of the total weight of the additive; the weight ratio of quartz sand is 25% of the total weight of the additive, and the particle size is 0.1mm<0.5mm; the weight ratio of dolomite is 25% of the total weight of the additive, and the particle size is 0.1mm<0.5mm;

[0072] The refractory coating 5 is prepared according to the following proportions:

[0073] 26 parts of aluminum oxide, 36 parts of calcium oxide, 35 parts of silica sol, and 3 parts of bentonite; mix them evenly and apply them on the surface of the ultrasonic probe, and dry them at 550°C for 1 hour.

[0074] The solid semicircular ring structure 2 and the hollow cylindrical structure 3 of the device for preventing the tundish upper water inlet from being blocked are manufactured by an integrated molding method according to the following process:

[0075] 1) Place 30 parts of flake graphite, 28 parts of magnesite powder, 9 parts of silicon dioxide, 15 parts of magnesium oxide, and 18 parts of additives in a container and vibrate it up and down and left and right.

[0076] 2) Place the container on a vibration table, add epoxy resin, and turn on the vibration switch to vibrate it up and down and left and right in turn. The up and down vibration time is 20 minutes, and the horizontal vibration time is 20 minutes.

[0077] 3) Add the raw materials in the container into the mold and form it in a pressure sintering machine. The sintering pressure is continuously increased as the temperature rises. The final forming temperature is 1050° C. and the final forming pressure is 150 MPa.

[0078] 4) The formed device is cooled for 1.5 hours before fine processing. The coated ultrasonic probe 4, horn 6, and transducer 7 are placed into the hollow cylindrical structure 3. The transducer 7 is connected to the ultrasonic generator 9 via a wire 8.

[0079] After testing, the physical performance indicators of the solid semicircular structure 2 and the hollow cylindrical structure 3 of the device for preventing the tundish upper water inlet from being blocked are: volume density 4.9g / cm3 ; Raw material true density 5.1g / cm 3 ; Calculated relative density (bulk density / true density) = 96.1%; refractoriness 1799℃; room temperature flexural strength 25.1Mpa. This shows that the device has excellent density and thermal stability

[0080] During the continuous casting process of aluminum-killed steel, the device was applied to the tundish water inlet. The device had good thermal stability, the coating on the probe surface did not fall off and there was no corrosion. The number of continuous pouring furnaces was increased to 25, and the number of continuous pouring furnaces was greatly increased.

[0081] Embodiment 4:

[0082] The solid semicircular structure 2 and the hollow cylindrical structure 3 are mixed according to the following weight ratio:

[0083] 31 parts of flake graphite, 29 parts of magnesite powder, 5 parts of silicon dioxide, 20 parts of magnesium oxide, 15 parts of additives and 10 parts of epoxy resin;

[0084] The additive is composed of clay, quartz sand and dolomite, wherein the weight ratio of clay is 30% of the total weight of the additive; the weight ratio of quartz sand is 40% of the total weight of the additive, with a particle size of 0.1 mm < 0.5 mm; the weight ratio of dolomite is 30% of the total weight of the additive, with a particle size of 0.1 mm < 0.5 mm;

[0085] The refractory coating 5 is prepared according to the following proportions:

[0086] 28 parts of aluminum oxide, 40 parts of calcium oxide, 30 parts of silica sol, and 2 parts of bentonite; mix them evenly and apply them on the surface of the ultrasonic probe 4, and dry them at 590°C for 1 hour.

[0087] The solid semicircular ring structure 2 and the hollow cylindrical structure 3 of the device for preventing the tundish upper water inlet from being blocked are manufactured by an integrated molding method according to the following process:

[0088] 1) 31 parts of flake graphite, 29 parts of magnesite powder, 5 parts of silicon dioxide, 20 parts of magnesium oxide, and 15 parts of additives are placed in a container and vibrated up and down and left and right.

[0089] 2) Place the container on a vibration table, add epoxy resin, and turn on the vibration switch to vibrate it up and down and left and right in turn. The up and down vibration time is 20 minutes, and the horizontal vibration time is 20 minutes.

[0090] 3) Add the raw materials in the container into the mold and form it in a pressure sintering machine. The sintering pressure is continuously increased as the temperature rises. The final forming temperature is 1040° C. and the final forming pressure is 150 MPa.

[0091] 4) The formed device is cooled for 1.5 hours before fine processing. The coated ultrasonic probe 4, horn 6, and transducer 7 are placed into the hollow cylindrical structure 3. The transducer 7 is connected to the ultrasonic generator 9 via a wire 8.

[0092] After testing, the physical performance indicators of the solid semicircular structure 2 and the hollow cylindrical structure 3 of the device for preventing the tundish upper water inlet from being blocked are: volume density 4.7g / cm 3 ; Raw material true density 5.0g / cm 3 ; Calculated relative density (bulk density / true density) = 94.0%; refractoriness 1829℃; room temperature flexural strength 24.0Mpa. This shows that the device has excellent density and thermal stability

[0093] During the continuous casting process of aluminum-killed steel, the device was applied to the tundish water inlet. The device had good thermal stability, the coating on the probe surface did not fall off and there was no corrosion. The number of continuous pouring furnaces was increased to 21, and the number of continuous pouring furnaces was greatly increased.

Claims

1. A method for manufacturing a device for preventing tundish water inlet from being blocked, characterized in that: The device comprises a solid semicircular ring structure (2), a hollow cylindrical structure (3), an ultrasonic probe (4), a horn (6), and a transducer (7); the hollow cylindrical structure (3) is integrally connected to the solid semicircular ring structure; the inner arc of the solid semicircular ring structure matches the outer arc of the nozzle; the interior of the hollow cylindrical structure is connected in sequence with the ultrasonic probe (4), the horn (6), and the transducer (7); the transducer (7) is connected to an ultrasonic generator (9) via a wire (8); and the surface of the ultrasonic probe (4) is covered with a refractory coating (5); The solid semicircular ring structure (2) and the hollow cylindrical structure (3) are prepared from the following raw materials in parts by weight: 30-35 parts of flake graphite, 20-30 parts of magnesite powder, 5-10 parts of silicon dioxide, 15-20 parts of magnesium oxide, 5-15 parts of additives, and 8-10 parts of epoxy resin; The solid semicircular ring structure (2) and the hollow cylindrical structure (3) of the device are formed in one piece, and the specific method includes: 1) Put flake graphite, magnesia powder, silicon dioxide, magnesium oxide and additives into a container and place it on a vibration table for vibration; 2) Add epoxy resin into the container, turn on the vibration switch, and make it vibrate up and down and horizontally in sequence. The up and down vibration time is 10 to 30 minutes, and the horizontal vibration time is 10 to 30 minutes; 3) Add the raw materials in the container into the mold and form it in a pressure sintering machine. As the temperature rises, the sintering pressure is continuously increased. The final molding temperature is 950-1300°C and the final molding pressure is 150MPa-180MPa. 4) The integrally formed solid semicircular ring structure (2) and hollow cylindrical structure (3) are cooled for 1 to 2 hours before being fine-processed, and the ultrasonic probe (4), horn (6), and transducer (7) coated with a fire-resistant coating are placed into the hollow cylindrical structure (3), and the transducer (7) is connected to the ultrasonic generator (9) via a wire (8).

2. The method for manufacturing a device for preventing tundish water outlet from being blocked according to claim 1, characterized in that: The two groups of devices for preventing the tundish water outlet from being blocked are mounted on the outer side of the water outlet in a buckled manner.

3. The method for manufacturing a device for preventing tundish water outlet from being blocked according to claim 1, characterized in that: The additive is one or a combination of clay, quartz sand and dolomite.

4. The method for manufacturing a device for preventing tundish water outlet from being blocked according to claim 1, characterized in that: The refractory coating (5) is prepared from the following raw materials in parts by weight: 20-40 parts of aluminum oxide, 30-45 parts of calcium oxide, 30-35 parts of silica sol, and 0-3 parts of bentonite.

5. The method for manufacturing a device for preventing tundish water outlet from being blocked according to claim 4, characterized in that: The method for preparing the refractory coating is as follows: the raw materials of the refractory coating are mixed evenly, then applied on the surface of the ultrasonic probe, and dried at a temperature of 520°C to 600°C for 1h to 2h.

Citation Information

Patent Citations

  • Anti-plugging tundish water supplying opening and manufacturing method thereof

    CN102416451B

  • Method for removing slag inclusion of continuous casting tundish purging upper nozzle seating brick through argon blowing

    CN107321945A

  • Multifunctional continuous casting tundish upper nozzle

    CN213257089U

  • Method of improving molten steel cleanness and refining crystal grains with ultrasonic waves

    CN103252459A

  • Method for preventing clogging of immersion nozzle

    JP1983151949A