A method for preparing aluminum-clad ceramic film circuit board
By forming a Ti layer on the ceramic substrate and using Al/Zn alloy wettability sintering, the problem of surface defects of the aluminum-coated ceramic film circuit board during the high-temperature sintering process is solved, a highly reliable aluminum-ceramic connection is achieved, and the circuit efficiency is significantly improved. Thermal cycling reliability and quality of the board.
Patent Information
- Application Number
- CN202410227510.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-02-29
AI Technical Summary
Aluminum-coated ceramic film circuit boards are prone to surface defects such as shrinkage holes and bulges during high-temperature sintering, resulting in low yields and insufficient bonding with ceramic substrates, affecting their reliability and service life.
Vacuum magnetron sputtering is used to form a Ti layer on the ceramic substrate, and Al/Zn alloy slurry is used for metallization. Highly reliable connection between aluminum and ceramics is achieved under low temperature conditions through wettability sintering, utilizing the volatility of the Zn element. Accelerate the melting, solidification and cooling process under high temperature vacuum conditions and eliminate surface defects.
It significantly enhances the thermal cycle reliability of the aluminum-coated ceramic film circuit board, eliminates surface defects such as shrinkage holes and bulges in the aluminum metallization layer after sintering, and improves the quality and performance of the circuit board.
Smart Images

Figure CN117956696B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor packaging, and in particular to a method for preparing an aluminum-clad ceramic film circuit board. Background Art
[0002] Ceramic thin film circuit substrate is a widely used electronic component substrate material. With its high integration, small size, high dimensional accuracy and other characteristics, it is mostly used in high-frequency and high-power occasions.
[0003] After the copper-clad ceramic film circuit board is sputtered with a copper seed layer on the ceramic substrate, a plating process is used to complete the preparation of the electrical circuit. However, the bonding force with the substrate is weak, which reduces the service life of the film circuit board and affects its reliability.
[0004] In contrast, aluminum-clad ceramic circuit boards can significantly enhance the heat-resistant cycle reliability of the substrate, thereby extending its life, because the aluminum layer has a smaller yield stress and better plasticity. However, aluminum has poor wettability on ceramics, and the sintering temperature needs to reach above 900°C. During the high-temperature sintering and cooling process, the aluminum-clad liquid surface is prone to shrinkage, forming defects such as shrinkage cavities and bulges, resulting in a low yield rate. The difficulty in preparing aluminum-clad ceramic thin film circuit boards lies mainly in the fact that during the high-temperature sintering and solidification process, the aluminum melt solidifies unevenly on the surface, resulting in surface defects such as shrinkage cavities and bulges.
[0005] Therefore, we propose a method for preparing an aluminum-clad ceramic film circuit board. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing an aluminum-clad ceramic thin film circuit board to solve the problems raised in the above background technology.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0008] A method for preparing an aluminum-clad ceramic film circuit board comprises the following steps:
[0009] Step 1: Ceramic substrate metallization: A Ti layer is sputtered on the upper and lower surfaces of the ceramic substrate by vacuum magnetron sputtering; Al / Zn alloy slurry is coated on the Ti layer by screen printing, and then dried to form an aluminum alloy metallization layer;
[0010] Step 2: Wetting sintering: Take the ceramic substrate obtained in step 1, put it into a vacuum furnace for wetting sintering, and take it out of the furnace after cooling to obtain an aluminum metallization layer;
[0011] Step 3: Etching electrical circuits: The surface of the ceramic substrate obtained in step 2 is covered with a photosensitive dry film, the surface of the photosensitive dry film is patterned, and the surface of the photosensitive dry film is developed, etched, stripped, cleaned, and dried in sequence to obtain an etched aluminum film-covered circuit board.
[0012] Furthermore, the magnetron sputtering working conditions in step 1 are: sputtering power 3-7KW, argon flow rate 30-35sccm, sputtering pressure 0.1-0.4Pa, vacuum degree 5×10 -5 -1×10 -4 pa.
[0013] Furthermore, in the step 1, the thickness of the Ti layer is 10-80 nm.
[0014] Furthermore, in the step 1, the Al / Zn alloy slurry comprises the following components in percentage by mass: 70-80% alloy metal and 20-30% organic solvent.
[0015] Furthermore, the alloy metal includes the following components in mass percentage: 70-90% aluminum and 10-30% zinc.
[0016] Furthermore, the organic solvent is a mixture of one or more of anhydrous ethanol, isopropyl alcohol and terpineol.
[0017] Furthermore, the Al / Zn alloy slurry is stirred with a glass rod for 5-10 minutes, and then ground with a three-roll grinder for 4-6 times.
[0018] Furthermore, the screen printing process conditions in step 1 are: printing mesh size 300-500 mesh.
[0019] Furthermore, the drying process conditions in step 1 are: drying temperature 110-140° C., and drying time 20-40 min.
[0020] Furthermore, in the step 1, the thickness of the aluminum alloy metallization layer is 10-15 μm.
[0021] Furthermore, the wettability sintering process conditions in step 2 are: sintering temperature 580-600°C, under nitrogen protection conditions, keeping warm for 1.5-2.0h at a vacuum degree of 100-150Pa, and keeping warm for 2-4h at a vacuum degree of 0.1-5.0Pa.
[0022] Furthermore, the surface component of the aluminum metallization layer after sintering in step 2 is high-purity aluminum, including the following components in weight percentage: Al≥99.8%, Zn≤0.1%, and other elements≤0.1%.
[0023] Furthermore, in the step 2, the thickness of the aluminum metallization layer is 5-10 μm.
[0024] Furthermore, in step three, 5-10 wt % sodium hydroxide solution is used to remove the film.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The present invention provides a method for preparing an aluminum-clad ceramic thin film circuit board, which metalizes the surface of a ceramic substrate to enhance the wettability of aluminum metal and ceramic, thereby forming a uniform and highly reliable film; the present invention innovatively uses Al / Zn alloy slurry to reduce the melting point of aluminum metal, thereby achieving high-reliability infiltration connection of Al and ceramic under low-temperature sintering conditions (<660°C). At the same time, under high-temperature vacuum conditions, the Zn element has strong volatility, and after a period of heat preservation, high-purity aluminum and ceramic can be bonded, thereby preparing an aluminum-based ceramic thin film circuit board motherboard; compared with the preparation method of copper-clad ceramic thin film circuit boards, the preparation method of the present invention significantly enhances the thermal cycle reliability of aluminum-clad ceramic thin film circuit boards.
[0027] 2. The method for preparing an aluminum-clad ceramic thin film circuit board of the present invention utilizes the heat-absorbing characteristics of the molten metal of the Zn element when the Al / Zn alloy slurry is in a molten state, which has a low boiling point and is easily volatile in a vacuum. This can significantly accelerate the melting, solidification and cooling process, eliminate surface defects caused by shrinkage tension, and successfully solve the surface defect problems such as shrinkage cavities and ridges of the aluminum metallization layer after sintering, and can efficiently prepare aluminum-clad ceramic thin film circuit boards. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0029] Figure 1 It is a process flow chart of an embodiment of the present invention;
[0030] Figure 2 This is an overall diagram of the aluminum film-covered circuit board before etching in Example 1 of the present invention;
[0031] Figure 3 This is a partial enlarged view of the aluminum film-covered circuit board after etching in Example 1 of the present invention;
[0032] Figure 4 This is an overall view of the aluminum film-coated circuit board before etching in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] In this embodiment, the Ti target: item number DCTI001, titanium content ≥99.99%, sourced from Suzhou Dongchen Xianrui New Material Technology Co., Ltd.; high-purity aluminum metal powder: particle size is 325 mesh, aluminum content ≥99.9%, sourced from Beijing Yijin New Material Technology Co., Ltd.; high-purity zinc metal powder: particle size is 325 mesh, zinc content ≥99.5%, sourced from Shijiazhuang Xinri Zinc Industry Co., Ltd.; wire mesh: 300-500 mesh, sourced from Shijiazhuang Chixin Wire Mesh Co., Ltd.; photosensitive dry film: model HT-115, sourced from Huizhou Dingbang Electronics Co., Ltd.
[0035] Embodiment 1: A method for preparing an aluminum-clad ceramic film circuit board, comprising the following steps:
[0036] Step 1: Ceramic substrate metallization: vacuum magnetron sputtering method, using pure metal target Ti target, sputtered a layer of Ti with a thickness of 50nm on the upper and lower surfaces of the ceramic substrate (sputtering power 3KW, argon flow rate 30sccm, sputtering pressure 0.1Pa, vacuum degree 5×10 -5 pa); 67g of high-purity aluminum metal powder and 8g of high-purity zinc metal powder were mixed evenly to obtain an alloy metal, and then 25g of pine alcohol organic solvent was added to mix, stirred with a glass rod for 5min, and then ground with a three-roll grinder for 4 times to obtain an Al / Zn alloy slurry; the Al / Zn alloy slurry was coated on the Ti layer using a 300-mesh screen, and then dried (drying temperature 120°C, drying time 30min) to form an aluminum alloy metallization layer with a thickness of 10μm;
[0037] Step 2: Wetting sintering: Take the ceramic substrate obtained in step 1 and put it into a vacuum furnace for wetting sintering. The sintering temperature is 580°C. Under nitrogen protection, keep it warm for 1.5 hours at a vacuum degree of 100Pa and keep it warm for 2 hours at a vacuum degree of 0.1Pa. Then cool it down and take it out of the furnace to form an aluminum metallization layer with a thickness of 5μm, and obtain an aluminum film-coated circuit board before etching.
[0038] Step 3: Etching electrical circuits: The surface of the ceramic substrate obtained in step 2 is covered with a photosensitive dry film, the surface of the photosensitive dry film is patterned, and the surface of the photosensitive dry film is developed and etched in turn, and a 5wt% sodium hydroxide solution is used to remove the film. After washing with deionized water, it is dried to obtain an etched aluminum film-covered circuit board.
[0039] Embodiment 2: A method for preparing an aluminum-clad ceramic film circuit board, comprising the following steps:
[0040] Step 1: Ceramic substrate metallization: vacuum magnetron sputtering method, using pure metal target Ti target, sputtered a layer of Ti with a thickness of 60nm on the upper and lower surfaces of the ceramic substrate (sputtering power 5KW, argon flow rate 32sccm, sputtering pressure 0.3Pa, vacuum degree 8×10 -5 pa); 81g of high-purity aluminum metal powder and 9g of high-purity zinc metal powder were mixed uniformly to obtain an alloy metal, and 23g of isopropanol organic solvent was added to mix, stirred with a glass rod for 8min, and then ground with a three-roll grinder for 4 times to obtain an Al / Zn alloy slurry; the Al / Zn alloy slurry was coated on the Ti layer using a 500-mesh screen, and then dried (drying temperature 110°C, drying time 40min) to form an aluminum alloy metallization layer with a thickness of 12μm;
[0041] Step 2: Wetting sintering: Take the ceramic substrate obtained in step 1, put it into a vacuum furnace for wetting sintering, the sintering temperature is 590°C, under nitrogen protection, keep it warm for 1.8 hours under a vacuum degree of 120Pa, keep it warm for 3 hours under a vacuum degree of 1Pa, cool it down and take it out of the furnace, forming an aluminum metallization layer with a thickness of 8μm, and obtaining an aluminum film-coated circuit board before etching;
[0042] Step 3: Etching electrical circuits: The surface of the ceramic substrate obtained in step 2 is covered with a photosensitive dry film, the surface of the photosensitive dry film is patterned, and the surface of the photosensitive dry film is developed and etched in turn, and an 8wt% sodium hydroxide solution is used to remove the film. After washing with deionized water, it is dried to obtain an etched aluminum film-covered circuit board.
[0043] Embodiment 3: A method for preparing an aluminum-clad ceramic film circuit board, comprising the following steps:
[0044] Step 1: Ceramic substrate metallization: vacuum magnetron sputtering method, using pure metal target Ti target, sputtered a layer of Ti with a thickness of 80nm on the upper and lower surfaces of the ceramic substrate (sputtering power 7KW, argon flow rate 35sccm, sputtering pressure 0.4Pa, vacuum degree 1×10 -4 pa); 85.5g of high-purity aluminum metal powder and 9.5g of high-purity zinc metal powder were mixed uniformly to obtain an alloy metal, and 32g of pine alcohol organic solvent was added to mix, stirred with a glass rod for 10min, and then ground with a three-roll grinder for 6 times to obtain an Al / Zn alloy slurry; the Al / Zn alloy slurry was coated on the Ti layer using a 400-mesh screen, and then dried (drying temperature 140°C, drying time 20min) to form an aluminum alloy metallization layer with a thickness of 15μm;
[0045] Step 2: Wetting sintering: Take the ceramic substrate obtained in step 1, put it into a vacuum furnace for wetting sintering, the sintering temperature is 600°C, under nitrogen protection, keep it warm for 2.0 hours at a vacuum degree of 150Pa, keep it warm for 4 hours at a vacuum degree of 5.0Pa, cool it down and take it out of the furnace, forming an aluminum metallization layer with a thickness of 10μm, and obtaining an aluminum film-coated circuit board before etching;
[0046] Step 3: Etching electrical circuits: The surface of the ceramic substrate obtained in step 2 is covered with a photosensitive dry film, the surface of the photosensitive dry film is patterned, and the surface of the photosensitive dry film is developed and etched in turn, and a 10wt% sodium hydroxide solution is used to remove the film. After washing with deionized water, it is dried to obtain an etched aluminum film-covered circuit board.
[0047] Comparative Example 1: A method for preparing an aluminum-clad ceramic film circuit board, comprising the following steps:
[0048] Compared with Example 1, in Comparative Example 1, the Al / Zn alloy slurry in step 1 is replaced with high-purity aluminum slurry of the same mass (85g high-purity aluminum metal powder, 25g pinene alcohol organic solvent), and the other steps are the same as those in Example 1.
[0049] Comparative Example 2: A method for preparing an aluminum-clad ceramic film circuit board, comprising the following steps:
[0050] Compared with Example 1, the Al / Zn alloy slurry in Comparative Example 2 includes the following components in mass percentage: 50% alloy metal and 50% organic solvent, and the other steps are the same as those in Example 1.
[0051] Comparative Example 3: A method for preparing an aluminum-clad ceramic film circuit board, comprising the following steps:
[0052] Compared with Example 1, the sintering temperature in step 2 of Comparative Example 3 is 520° C., and the other steps are the same as those of Example 1.
[0053] Comparative Example 4: A method for preparing an aluminum-clad ceramic film circuit board, comprising the following steps:
[0054] Compared with Example 1, the wettability sintering process conditions in step 2 of Comparative Example 4 are: the sintering temperature is 580°C, under nitrogen protection conditions, the sintering is carried out for 1.5 hours at a vacuum degree of 80Pa and for 2 hours at a vacuum degree of 10Pa, and the other steps are the same as in Example 1.
[0055] Experiment: The aluminum film-coated circuit boards before etching and the aluminum film-coated circuit boards after etching obtained in Examples 1-3 and Comparative Examples 1-4 were taken to prepare samples, and the appearance of the samples was tested and the test results were recorded:
[0056] Appearance inspection: Evaluate the quality and performance of the circuit board by observing whether the surface is flat and whether there are defects such as bulging, blistering, shrinkage, etc.
[0057] Test results:
[0058] Aluminum film PCB before etching Aluminum film PCB after etching Example 1 Smooth surface The edge of the aluminum layer is smooth, and no pattern spacing etching residue is seen Example 2 Smooth surface The edge of the aluminum layer is smooth, and no pattern spacing etching residue is seen Example 3 Smooth surface The edge of the aluminum layer is smooth, and no pattern spacing etching residue is seen Comparative Example 1 There are bulging and shrinkage phenomena The edge of the aluminum layer is uneven, and there is etching residue between the patterns. Comparative Example 2 There is a bulging phenomenon There is etching residue in the pattern spacing Comparative Example 3 There is shrinkage phenomenon There is etching residue in the pattern spacing Comparative Example 4 There is shrinkage phenomenon There is etching residue in the pattern spacing
[0059] According to the data in the above table, we can clearly draw the following conclusions:
[0060] 1. Compared with Examples 1-3, the aluminum film-coated circuit board of Comparative Example 1 still has surface defects before and after etching, indicating that, compared with high-purity aluminum paste, the Al / Zn alloy paste prepared by the present invention can eliminate surface defects caused by shrinkage tension.
[0061] 2. Compared with Examples 1-3, the aluminum-clad film circuit board of Comparative Example 2 still has defects on its surface before and after etching. It can be seen that the performance of the Al / Zn alloy slurry prepared by the present invention is affected by its component ratio. Selecting a component ratio within the said range can better achieve the bonding of the high-purity aluminum surface and the ceramic to eliminate surface defects.
[0062] 3. Compared with Examples 1-3, the aluminum film-clad circuit board of Comparative Example 3 still has defects on its surface before and after etching, indicating that lowering the sintering temperature will cause incomplete sintering of the film, thereby affecting the performance of the circuit board.
[0063] 4. Compared with Examples 1-3, the aluminum film-coated circuit board of Comparative Example 3 still has defects on its surface before and after etching, indicating that the performance of the aluminum metallization layer prepared by the present invention is affected by the vacuum degree in its wettability sintering process. Selecting process conditions within the said range can make the zinc element more volatilized, which is beneficial to solving the problem of surface defects after sintering and solidification.
[0064] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0065] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an aluminum-clad ceramic film circuit board, characterized in that: The following steps are involved: Step 1: Ceramic substrate metallization: A Ti layer is sputtered on the upper and lower surfaces of the ceramic substrate by vacuum magnetron sputtering; The Al / Zn alloy slurry is coated on the Ti layer by screen printing process, and then dried to form an aluminum alloy metallization layer; Step 2: Wetting sintering: Take the ceramic substrate obtained in step 1, put it into a vacuum furnace for wetting sintering, and take it out of the furnace after cooling to obtain an aluminum metallization layer; Step 3: Etching electrical circuits: The surface of the ceramic substrate obtained in step 2 is covered with a photosensitive dry film, the surface of the photosensitive dry film is patterned, and the surface of the photosensitive dry film is developed, etched, stripped, cleaned, and dried in sequence to obtain an etched aluminum film-covered circuit board; In the step 1, the Al / Zn alloy slurry comprises the following components in percentage by weight: 70-80% alloy metal and 20-30% organic solvent; The alloy metal comprises the following components in percentage by mass: 70-90% aluminum and 10-30% zinc; the organic solvent is a mixture of one or more of anhydrous ethanol, isopropyl alcohol and terpineol; The wettability sintering process conditions in the step 2 are: sintering temperature 580-600° C., under nitrogen protection, keeping warm for 1.5-2.0 hours at a vacuum degree of 100-150 Pa, and keeping warm for 2-4 hours at a vacuum degree of 0.1-5.0 Pa.
2. The method for preparing an aluminum-clad ceramic thin film circuit board according to claim 1, characterized in that: The magnetron sputtering working conditions in step 1 are: sputtering power 3-7KW, argon gas flow rate 30-35sccm, sputtering pressure 0.1-0.4Pa, vacuum degree 5×10 -5 -1×10 -4 pa.
3. The method for preparing an aluminum-clad ceramic thin film circuit board according to claim 1, characterized in that: The screen printing process conditions in step 1 are: printing mesh number 300-500 mesh.
4. The method for preparing an aluminum-clad ceramic thin film circuit board according to claim 1, characterized in that: The drying process conditions in step 1 are: drying temperature 110-140° C., and drying time 20-40 min.
5. The method for preparing an aluminum-clad ceramic thin film circuit board according to claim 1, characterized in that: The thickness of the aluminum alloy metallization layer in step 1 is 10-15 μm.
6. The method for preparing an aluminum-clad ceramic thin film circuit board according to claim 1, characterized in that: The thickness of the aluminum metallization layer in step 2 is 5-10 μm.
7. The method for preparing an aluminum-clad ceramic thin film circuit board according to claim 1, characterized in that: The surface composition of the aluminum metallization layer after sintering in step 2 is high-purity aluminum, including the following elements in weight percentage: Al≥99.8%, Zn≤0.1%, and other elements≤0.1%.
Citation Information
Patent Citations
Preparation method of ceramic aluminum-coated lining plate
CN113511915A
Aluminum oxide ceramic surface metallization method
CN114988918A
Ceramic heating sheet and preparation method thereof
CN116420927A
Preparation method of ceramic aluminum-coated substrate and ceramic aluminum-coated substrate prepared by same
CN116751070A
Ceramic container and battery and electric double layer capacitor using the same
US20060187614A1