Polyurethane-acrylate anticorrosive coating and preparation method thereof
By using modified preservatives and composite UV absorbers, combined with polyurethane and acrylate, the problem of insufficient corrosion resistance and weather resistance of polyurethane-acrylate anti-corrosion coatings is solved, and the excellent performance of the coatings in extreme environments is achieved.
Patent Information
- Application Number
- CN202411195304.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The corrosion resistance and weather resistance of existing polyurethane-acrylate anti-corrosion coatings are poor, making it difficult to meet the application needs in extreme environments.
Benzo[1,2-b:3,4-b':5,6-b'] trithiophene-2,5,8-trialdehyde and 1,3,5-tris(4-aminophenyl) were used Prepare modified preservatives by benzene, and prepare composite UV absorbers with para-aminobenzonitrile, dicyanide and terephthalaldehyde. Combining potassium persulfate, polyurethane and acrylate, polyurethane-acrylate anti-corrosion is prepared through specific process steps. coating.
The corrosion resistance and weather resistance of the coating are significantly improved. The π-electron system of modified thiophene rings and composite UV absorbers in the preservative can resist the degradation of ultraviolet rays and oxygen, extend the service life of the coating, and form a dense mesh. The structure and polymer chain cross-links enhance the corrosion resistance of the coating.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-corrosion coating preparation, and specifically relates to a polyurethane-acrylate anti-corrosion coating and a preparation method thereof. Background Art
[0002] With the continuous advancement of industrial technology, the requirements for coating performance are also increasing, especially in the field of anti-corrosion. Traditional coatings can no longer meet the stringent requirements for durability, weather resistance and corrosion resistance in extreme environments. Since its discovery in the 1950s, polyurethane, as an important polymer material, has rapidly expanded its application to many industries such as construction, automobiles, aerospace, and medical devices. Polyurethane materials are known for their excellent mechanical properties, wear resistance, chemical resistance, and good processing properties. However, when polyurethane materials are used alone, their anti-corrosion performance is still insufficient in certain specific applications, such as marine environments and chemical industries. At the same time, polyacrylates, as another important class of polymer materials, have a place in the coating field with their excellent weather resistance, water resistance, and gloss. The quick drying and good film-forming properties of polyacrylate coatings make them perform well in outdoor coatings. However, their relatively weak hardness and wear resistance limit their application in high-load or high-wear environments.
[0003] Polyurethane-acrylate composite emulsion came into being in this context. The composite emulsion not only retains the excellent mechanical properties, wear resistance and chemical resistance of polyurethane materials, but also integrates the weather resistance, glossiness and quick drying of polyacrylates, thereby significantly improving the comprehensive performance of the coating.
[0004] Patent CN 104031231 A discloses a UV-curable waterborne epoxy-polyurethane-acrylate copolymer resin-based anticorrosive coating and a preparation method thereof. The resin is polymerized by three monomers, namely epoxy resin, polyurethane and acrylic resin, and the base resin is self-emulsified in water to obtain an epoxy-polyurethane-acrylate copolymer resin aqueous dispersion. A waterborne photoinitiator, an acrylate crosslinking agent and other auxiliary agents are added to the aqueous dispersion to obtain a UV-curable waterborne epoxy-polyurethane-acrylate copolymer resin-based anticorrosive coating. The synthesis process is simple, the coating uses water as a dispersion medium, and the cured coating of the anticorrosive coating has good adhesion, hardness, gloss and corrosion resistance. However, the corrosion resistance and weather resistance of the coating prepared by this method still have room for improvement. Summary of the invention
[0005] The purpose of the present invention is to provide a polyurethane-acrylate anticorrosive coating and a preparation method thereof, so as to solve the technical problem that the coating in the prior art has poor anticorrosion performance and poor weather resistance.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The invention provides a polyurethane-acrylate anticorrosive coating, which is composed of the following components in parts by weight: 30-45 parts of polyurethane, 10-15 parts of acrylate, 0.08-0.12 parts of potassium persulfate, 40-50 parts of deionized water, 3-6 parts of modified preservatives, and 2-4 parts of composite ultraviolet absorbers, wherein the modified preservative is prepared from benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and 1,3,5-tris(4-aminophenyl)benzene, and the composite ultraviolet absorber is prepared from p-aminobenzonitrile, 4-fluorobenzonitrile, dicyandiamide and terephthalaldehyde.
[0008] Preferably, the method for preparing the modified preservative comprises the following steps:
[0009] Q1: Add benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and 1,3,5-tris(4-aminophenyl)benzene to an ampoule, then add 1,3,5-trimethylbenzene, 1,4-dioxane and acetonitrile, mix by ultrasonication, add trifluoroacetic acid, and continue ultrasonication;
[0010] Q2: After the ultrasonic mixing, the ampoule is degassed by freeze-vacuum-thaw cycle, and then the ampoule is sealed and heated for reaction. After the reaction is completed, the ampoule is opened, washed, soaked, filtered, and vacuum dried to obtain a modified preservative.
[0011] In the above process, the synthetic reaction formula of the modified preservative is as follows:
[0012]
[0013] Preferably, in Q1, the usage ratio of benzo[1,2-b:3,4-b':5,6-b']trithiophene-2,5,8-trialdehyde, 1,3,5-tris(4-aminophenyl)benzene, 1,3,5-trimethylbenzene, 1,4-dioxane, acetonitrile and trifluoroacetic acid is (123.9-185.9) mg: (87.86-131.79) mg: (0.6-0.9) mL: (1.2-1.8) mL: (0.025-0.0375) mL: (0.2-0.3) mL, The purity of benzo[1,2-b:3,4-b':5,6-b']trithiophene-2,5,8-trialdehyde is 97%, the purity of 1,3,5-tri(4-aminophenyl)benzene is 98%, the ultrasonic mixing time is 15-25 min, and the continued ultrasonic mixing time is 5-10 min; in Q2, the heating reaction temperature is 140-160°C, the reaction time is 70-72h, washing is carried out with N,N-dimethylformamide, soaking is carried out with formaldehyde, and the vacuum drying temperature is 70-90°C for 20-24h.
[0014] Preferably, the preparation method of the composite ultraviolet absorber comprises the following steps:
[0015] S1: Add p-aminobenzonitrile, N,N-dimethylformamide and cesium fluoride into a container, perform ultrasonic treatment, then add 4-fluorobenzonitrile under stirring, heat under argon atmosphere, condense and reflux, and after completion, cool, precipitate, filter, wash and vacuum dry to obtain compound 1;
[0016] S2: Add compound 1, dicyandiamide, potassium hydroxide and ethylene glycol methyl ether into a container, stir and mix evenly, heat in an oil bath, and condense under an argon atmosphere. After the reaction is completed, cool, sonicate, filter, and vacuum dry to obtain compound 2;
[0017] S3: Add compound 2, terephthalaldehyde and dimethyl sulfoxide into a container, evacuate, pass argon, heat in an oil bath, condense and stir. After completion, cool, filter, extract and vacuum dry to obtain a composite UV absorber.
[0018] In the above process, the synthesis reaction formula of the composite ultraviolet absorber is as follows:
[0019]
[0020] Preferably, in S1, the dosage ratio of p-aminobenzonitrile, N,N-dimethylformamide, cesium fluoride and 4-fluorobenzonitrile is (1.18-1.89) g: (50-80) mL: (6.04-9.66) g: (2.66-4.26) g, the heating temperature is 130-150°C, the condensation reflux time is 45-48h, the vacuum drying temperature is 80-90°C, and the time is 10-12h.
[0021] Preferably, in S2, the dosage ratio of compound 1, dicyandiamide, potassium hydroxide and ethylene glycol methyl ether is (5.38-9.14) g: (2.94-4.99) g: (0.55-0.94) g: (50-85) mL, the oil bath heating temperature is 150-160°C, the condensation reaction time is 20-24 h, formaldehyde is added during the ultrasonic process, first washed with distilled water and then filtered, then washed with methanol and filtered, the vacuum drying temperature is 80-90°C, and the time is 48-52 h.
[0022] Preferably, in S3, the amount ratio of compound 2, terephthalaldehyde and dimethyl sulfoxide is (9.96-12.95) g: (2.68-3.48) g: (200-260) mL, the oil bath heating temperature is 180°C, and the condensation stirring time is 48-52 h. The oil bath heating process adopts a gradient temperature increase, and in the process of rising from room temperature to 50°C, 80°C, 110°C, and 140°C, each is maintained for 5 minutes, and finally the temperature is raised to 180°C, and methanol, tetrahydrofuran and dichloromethane are each extracted for 12 hours, and the vacuum drying temperature is 140-160°C for 20-24 hours.
[0023] Preferably, the method for preparing the polyurethane-acrylate anticorrosive coating comprises the following steps:
[0024] Step (1): firstly, potassium persulfate is added into deionized water to obtain a potassium persulfate solution, then the polyurethane is heated in a water bath, and then the acrylate and the potassium persulfate solution are gradually added dropwise into the polyurethane through a constant pressure funnel, the adding time is controlled, and after the adding is completed, the reaction is stirred to obtain a composite emulsion;
[0025] Step (2): adding the modified preservative and the composite ultraviolet absorber to the composite emulsion, stirring and mixing, standing, and vacuum drying to obtain a polyurethane-acrylate anticorrosive coating.
[0026] Preferably, in step (1), the water bath heating temperature is 80-90°C, the time is 5-8 min, the dripping time is controlled to be 1-1.5 h, the stirring time is 3-5 h, and the stirring speed is 400-600 rpm; in step (2), the mixing and stirring time is 1-2 h, the standing time is 20-24 h, and the vacuum drying temperature is 50-60°C, and the time is 12-18 h.
[0027] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0028] 1. The present invention uses benzo[1,2-b:3,4-b':5,6-b']trithiophene-2,5,8-trialdehyde and 1,3,5-tris(4-aminophenyl)benzene as raw materials to prepare a modified preservative, and then uses p-aminobenzonitrile, dicyandiamide and terephthalaldehyde as raw materials to prepare a composite ultraviolet absorber. The modified preservative and the composite ultraviolet absorber are added to the coating at the same time, so that the prepared polyurethane-acrylate anticorrosive coating has excellent corrosion resistance and weather resistance.
[0029] 2. The present invention uses benzo[1,2-b:3,4-b':5,6-b']trithiophene-2,5,8-trialdehyde and 1,3,5-tris(4-aminophenyl)benzene as raw materials to prepare a modified preservative. Adding the modified preservative to a coating can effectively improve the corrosion resistance and weather resistance of the coating. The thiophene ring contained in the modified preservative, as a heterocyclic structure, has excellent chemical stability and can resist degradation caused by environmental factors such as ultraviolet rays and oxygen, thereby extending the service life of the coating. The modified preservative can form a dense network structure in the coating, which can block the penetration of harmful substances such as moisture and oxygen, and further enhance the weather resistance of the coating. The stable chemical bonds formed in the modified preservative can exist in the coating and can firmly adhere to the surface of the substrate to form a protective film. The protective film not only has a physical barrier effect, but also can form a complex network structure through the entanglement and cross-linking of molecular chains, effectively preventing the invasion of microorganisms, corrosive media, etc., and improving the corrosion resistance of the coating.
[0030] 3. The present invention uses p-aminobenzonitrile, dicyandiamide and terephthalaldehyde as raw materials to prepare a composite ultraviolet absorber. The triazine structure and benzene ring contained in the structure work together, and the π electron system contained in the structure can absorb ultraviolet light energy and convert it into heat energy or other forms of energy dissipation to prevent ultraviolet rays from damaging the coating and the substrate it protects. The composite ultraviolet absorber has high thermal stability and chemical stability, can maintain its ultraviolet absorption performance in various environments, and delay the aging phenomena of the coating such as oxidation, yellowing, and cracking. The composite ultraviolet absorber can also enhance the cohesion and adhesion of the coating and improve the weather resistance of the coating through the entanglement and cross-linking of its polymer chains. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0032] This embodiment discloses a method for preparing a modified preservative, comprising the following steps:
[0033] Q1: 154.9 mg of 97% pure benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and 109.83 mg of 98% pure 1,3,5-tris(4-aminophenyl)benzene were added to an ampoule, followed by 0.75 mL of 1,3,5-tris(4-aminophenyl)benzene, 1.5 mL of 1,4-dioxane and 0.031 mL of acetonitrile. After ultrasonic mixing for 25 min, 0.25 mL of trifluoroacetic acid was added, and ultrasonic mixing was continued for 5 min.
[0034] Q2: After the ultrasonically mixed ampoule is degassed through a freeze-vacuum-thaw cycle, the ampoule is sealed and heated at 150°C for 72 hours. After the reaction is completed, the ampoule is opened, washed with N,N-dimethylformamide, soaked with formaldehyde, filtered, and vacuum dried at 80°C for 24 hours to obtain a modified preservative.
[0035] This embodiment discloses a method for preparing a composite ultraviolet absorber, comprising the following steps:
[0036] S1: 1.54 g of p-aminobenzonitrile, 65 mL of N,N-dimethylformamide and 7.85 g of cesium fluoride were added to a container, and ultrasonic treatment was performed. Then, 3.46 g of 4-fluorobenzonitrile was added under stirring. The mixture was heated at 140° C. under argon atmosphere, and condensed and refluxed for 48 h. After the reaction was completed, the mixture was cooled, precipitated, filtered, washed, and dried under vacuum at 80° C. for 12 h to obtain compound 1;
[0037] S2: 7.26 g of compound 1, 3.87 g of dicyandiamide, 0.75 g of potassium hydroxide and 67.5 mL of ethylene glycol methyl ether were added to a container, stirred and mixed evenly, heated in an oil bath at 160°C, and condensed under an argon atmosphere for 24 hours. After completion, the mixture was cooled, and formaldehyde was added for ultrasonication. The mixture was first washed with distilled water and then filtered, and then washed with methanol and filtered, and dried in a vacuum at 80°C for 48 hours to obtain compound 2;
[0038] S3: Add 11.45g of compound 2, 3.08g of terephthalaldehyde and 230mL of dimethyl sulfoxide into a container, evacuate, pass argon, and heat in an oil bath at 180°C. The oil bath heating process adopts a gradient temperature increase, and the temperature is maintained at 50°C, 80°C, 110°C, and 140°C for 5 minutes each. Finally, the temperature is increased to 180°C, condensed and stirred for 48 hours. After the temperature is reached, it is cooled, filtered, extracted with methanol, tetrahydrofuran and dichloromethane for 12 hours each, and dried in a vacuum at 160°C for 24 hours to obtain a composite ultraviolet absorber.
[0039] The present embodiment discloses a polyurethane-acrylate anticorrosive coating, which is composed of the following ingredients in parts by weight: 37.5 parts of polyurethane, 12.5 parts of acrylate, 0.1 parts of potassium persulfate, 45 parts of deionized water, 4.5 parts of modified preservative, and 3 parts of composite ultraviolet absorber.
[0040] This embodiment discloses a method for preparing a polyurethane-acrylate anticorrosive coating, comprising the following steps:
[0041] Step (1): first, potassium persulfate is added to deionized water to obtain a potassium persulfate solution, and then the polyurethane is heated in a water bath at 85° C. for 5 min, and then the acrylate and potassium persulfate solution are gradually added dropwise to the polyurethane through a constant pressure funnel, and the dropping time is controlled to be 1 h. After the dropping is completed, the reaction is stirred at 400 rpm for 5 h to obtain a composite emulsion;
[0042] Step (2): Add the modified preservative and the composite UV absorber to the composite emulsion, stir and mix for 2 hours, let stand for 24 hours, and vacuum dry at 60° C. for 18 hours to obtain a polyurethane-acrylate anticorrosive coating. Example 2
[0043] This embodiment discloses a method for preparing a modified preservative, comprising the following steps:
[0044] Q1: 123.9 mg of 97% pure benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and 87.86 mg of 98% pure 1,3,5-tris(4-aminophenyl)benzene were added to an ampoule, followed by 0.6 mL of 1,3,5-trisbenzene, 1.2 mL of 1,4-dioxane and 0.025 mL of acetonitrile. After ultrasonic mixing for 25 min, 0.2 mL of trifluoroacetic acid was added, and ultrasonic mixing was continued for 5 min.
[0045] Q2: After the ultrasonically mixed ampoule is degassed through a freeze-vacuum-thaw cycle, the ampoule is sealed and heated at 150°C for 72 hours. After the reaction is completed, the ampoule is opened, washed with N,N-dimethylformamide, soaked with formaldehyde, filtered, and vacuum dried at 80°C for 24 hours to obtain a modified preservative.
[0046] This embodiment discloses a method for preparing a composite ultraviolet absorber, comprising the following steps:
[0047] S1: 1.18 g of p-aminobenzonitrile, 50 mL of N,N-dimethylformamide and 6.04 g of cesium fluoride were added to a container, and ultrasonic treatment was performed. Then, 2.66 g of 4-fluorobenzonitrile was added under stirring. The mixture was heated at 140° C. under argon atmosphere, and refluxed under condensation for 48 h. After the mixture was cooled, precipitated, filtered, washed, and dried under vacuum at 80° C. for 12 h to obtain compound 1;
[0048] S2: Add 5.38g of compound 1, 2.94g of dicyandiamide, 0.55g of potassium hydroxide and 50mL of ethylene glycol methyl ether into a container, stir and mix evenly, heat in an oil bath at 160°C, and condense and react for 24h under an argon atmosphere. After the reaction, cool, add formaldehyde and perform ultrasound. First, wash with distilled water and filter, then wash with methanol and filter, and dry in a vacuum at 80°C for 48h to obtain compound 2;
[0049] S3: Add 9.96g of compound 2, 2.68g of terephthalaldehyde and 200mL of dimethyl sulfoxide into a container, evacuate, pass argon, and heat in an oil bath at 180°C. The oil bath heating process adopts a gradient temperature increase, and the temperature is maintained at 50°C, 80°C, 110°C, and 140°C for 5 minutes each. Finally, the temperature is increased to 180°C, condensed and stirred for 48 hours. After the temperature is reached, it is cooled, filtered, extracted with methanol, tetrahydrofuran and dichloromethane for 12 hours each, and dried in a vacuum at 160°C for 24 hours to obtain a composite ultraviolet absorber.
[0050] The present embodiment discloses a polyurethane-acrylate anticorrosive coating, which is composed of the following ingredients in parts by weight: 30 parts of polyurethane, 10 parts of acrylate, 0.08 parts of potassium persulfate, 40 parts of deionized water, 3 parts of modified preservative, and 2 parts of composite ultraviolet absorber.
[0051] This embodiment discloses a method for preparing a polyurethane-acrylate anticorrosive coating, comprising the following steps:
[0052] Step (1): first, potassium persulfate is added to deionized water to obtain a potassium persulfate solution, and then the polyurethane is heated in a water bath at 85° C. for 5 min, and then the acrylate and potassium persulfate solution are gradually added dropwise to the polyurethane through a constant pressure funnel, and the dropping time is controlled to be 1 h. After the dropping is completed, the reaction is stirred at 400 rpm for 5 h to obtain a composite emulsion;
[0053] Step (2): Add the modified preservative and the composite UV absorber to the composite emulsion, stir and mix for 2 hours, let stand for 24 hours, and vacuum dry at 60° C. for 18 hours to obtain a polyurethane-acrylate anticorrosive coating. Example 3
[0054] This embodiment discloses a method for preparing a modified preservative, comprising the following steps:
[0055] Q1: 185.9 mg of 97% pure benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and 131.79 mg of 98% pure 1,3,5-tris(4-aminophenyl)benzene were added to an ampoule, followed by 0.9 mL of 1,3,5-trimethylbenzene, 1.8 mL of 1,4-dioxane and 0.037 mL of acetonitrile. After ultrasonic mixing for 25 min, 0.3 mL of trifluoroacetic acid was added, and ultrasonic mixing was continued for 5 min.
[0056] Q2: After the ultrasonically mixed ampoule is degassed through a freeze-vacuum-thaw cycle, the ampoule is sealed and heated at 150°C for 72 hours. After the reaction is completed, the ampoule is opened, washed with N,N-dimethylformamide, soaked with formaldehyde, filtered, and vacuum dried at 80°C for 24 hours to obtain a modified preservative.
[0057] This embodiment discloses a method for preparing a composite ultraviolet absorber, comprising the following steps:
[0058] S1: 1.89 g of p-aminobenzonitrile, 80 mL of N,N-dimethylformamide and 9.66 g of cesium fluoride were added to a container, and ultrasonic treatment was performed. Then, 4.26 g of 4-fluorobenzonitrile was added under stirring. The mixture was heated at 140° C. under argon atmosphere, and refluxed under condensation for 48 h. After the mixture was cooled, precipitated, filtered, washed, and dried under vacuum at 80° C. for 12 h to obtain compound 1;
[0059] S2: 9.14 g of compound 1, 4.99 g of dicyandiamide, 0.94 g of potassium hydroxide and 85 mL of ethylene glycol methyl ether were added to a container, stirred and mixed evenly, heated in an oil bath at 160°C, and condensed for 24 h under an argon atmosphere. After completion, the mixture was cooled, and formaldehyde was added for ultrasonication. The mixture was first washed with distilled water and then filtered, and then washed with methanol and filtered. The mixture was vacuum dried at 80°C for 48 h to obtain compound 2.
[0060] S3: Add 12.95g of compound 2, 3.48g of terephthalaldehyde and 260mL of dimethyl sulfoxide into a container, evacuate, pass argon, and heat in an oil bath at 180°C. The oil bath heating process adopts a gradient temperature increase, and the temperature is maintained at 50°C, 80°C, 110°C, and 140°C for 5 minutes each. Finally, the temperature is increased to 180°C, condensed and stirred for 48 hours. After the temperature is reached, it is cooled, filtered, extracted with methanol, tetrahydrofuran and dichloromethane for 12 hours each, and dried in a vacuum at 160°C for 24 hours to obtain a composite ultraviolet absorber.
[0061] The present embodiment discloses a polyurethane-acrylate anticorrosive coating, which is composed of the following ingredients in parts by weight: 45 parts of polyurethane, 15 parts of acrylate, 0.12 parts of potassium persulfate, 50 parts of deionized water, 6 parts of modified preservative, and 4 parts of composite ultraviolet absorber.
[0062] This embodiment discloses a method for preparing a polyurethane-acrylate anticorrosive coating, comprising the following steps:
[0063] Step (1): first, potassium persulfate is added to deionized water to obtain a potassium persulfate solution, and then the polyurethane is heated in a water bath at 85° C. for 5 min, and then the acrylate and potassium persulfate solution are gradually added dropwise to the polyurethane through a constant pressure funnel, and the dropping time is controlled to be 1 h. After the dropping is completed, the reaction is stirred at 400 rpm for 5 h to obtain a composite emulsion;
[0064] Step (2): Add the modified preservative and the composite UV absorber to the composite emulsion, stir and mix for 2 hours, let stand for 24 hours, and vacuum dry at 60° C. for 18 hours to obtain a polyurethane-acrylate anticorrosive coating. Example 4
[0065] This embodiment discloses a method for preparing a modified preservative, comprising the following steps:
[0066] Q1: 139.4 mg of 97% pure benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and 98.85 mg of 98% pure 1,3,5-tris(4-aminophenyl)benzene were added to an ampoule, followed by 0.7 mL of 1,3,5-trisbenzene, 1.4 mL of 1,4-dioxane and 0.027 mL of acetonitrile. After ultrasonic mixing for 25 min, 0.22 mL of trifluoroacetic acid was added, and ultrasonic mixing was continued for 5 min.
[0067] Q2: After the ultrasonically mixed ampoule is degassed through a freeze-vacuum-thaw cycle, the ampoule is sealed and heated at 150°C for 72 hours. After the reaction is completed, the ampoule is opened, washed with N,N-dimethylformamide, soaked with formaldehyde, filtered, and vacuum dried at 80°C for 24 hours to obtain a modified preservative.
[0068] This embodiment discloses a method for preparing a composite ultraviolet absorber, comprising the following steps:
[0069] S1: 1.36 g of p-aminobenzonitrile, 60 mL of N,N-dimethylformamide and 6.95 g of cesium fluoride were added to a container, and ultrasonic treatment was performed. Then, 3.06 g of 4-fluorobenzonitrile was added under stirring. The mixture was heated at 140° C. under argon atmosphere, and condensed and refluxed for 48 h. After the reaction was completed, the mixture was cooled, precipitated, filtered, washed, and dried under vacuum at 80° C. for 12 h to obtain compound 1;
[0070] S2: Add 6.37 g of compound 1, 3.41 g of dicyandiamide, 0.65 g of potassium hydroxide and 58.8 mL of ethylene glycol methyl ether into a container, stir and mix evenly, heat in an oil bath at 160°C, and condense and react for 24 hours under an argon atmosphere. After the reaction is completed, cool, add formaldehyde and perform ultrasound. First, wash with distilled water and filter, then wash with methanol and filter, and dry in a vacuum at 80°C for 48 hours to obtain compound 2;
[0071] S3: Add 12.2g of compound 2, 2.88g of terephthalaldehyde and 215mL of dimethyl sulfoxide into a container, evacuate, pass argon, and heat in an oil bath at 180°C. The oil bath heating process adopts a gradient temperature increase, and the temperature is maintained at 50°C, 80°C, 110°C, and 140°C for 5 minutes each. Finally, the temperature is increased to 180°C, condensed and stirred for 48 hours. After the temperature is reached, cool and filter, extract with methanol, tetrahydrofuran and dichloromethane for 12 hours each, and vacuum dry at 160°C for 24 hours to obtain a composite ultraviolet absorber.
[0072] The present embodiment discloses a polyurethane-acrylate anticorrosive coating, which is composed of the following ingredients in parts by weight: 35 parts of polyurethane, 11 parts of acrylate, 0.09 parts of potassium persulfate, 42 parts of deionized water, 4 parts of modified preservative, and 2.5 parts of composite ultraviolet absorber.
[0073] This embodiment discloses a method for preparing a polyurethane-acrylate anticorrosive coating, comprising the following steps:
[0074] Step (1): first, potassium persulfate is added to deionized water to obtain a potassium persulfate solution, and then the polyurethane is heated in a water bath at 85° C. for 5 min, and then the acrylate and potassium persulfate solution are gradually added dropwise to the polyurethane through a constant pressure funnel, and the dropping time is controlled to be 1 h. After the dropping is completed, the reaction is stirred at 400 rpm for 5 h to obtain a composite emulsion;
[0075] Step (2): Add the modified preservative and the composite UV absorber to the composite emulsion, stir and mix for 2 hours, let stand for 24 hours, and vacuum dry at 60° C. for 18 hours to obtain a polyurethane-acrylate anticorrosive coating. Example 5
[0076] This embodiment discloses a method for preparing a modified preservative, comprising the following steps:
[0077] Q1: 170.4 mg of 97% pure benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and 120.81 mg of 98% pure 1,3,5-tris(4-aminophenyl)benzene were added to an ampoule, followed by 0.8 mL of 1,3,5-tris(4-aminophenyl)benzene, 1.7 mL of 1,4-dioxane and 0.034 mL of acetonitrile. After ultrasonic mixing for 25 min, 0.27 mL of trifluoroacetic acid was added, and ultrasonic mixing was continued for 5 min.
[0078] Q2: After the ultrasonically mixed ampoule is degassed through a freeze-vacuum-thaw cycle, the ampoule is sealed and heated at 150°C for 72 hours. After the reaction is completed, the ampoule is opened, washed with N,N-dimethylformamide, soaked with formaldehyde, filtered, and vacuum dried at 80°C for 24 hours to obtain a modified preservative.
[0079] This embodiment discloses a method for preparing a composite ultraviolet absorber, comprising the following steps:
[0080] S1: 1.72 g of p-aminobenzonitrile, 70 mL of N,N-dimethylformamide and 8.76 g of cesium fluoride were added to a container, and ultrasonic treatment was performed. Then, 3.86 g of 4-fluorobenzonitrile was added under stirring. The mixture was heated at 140° C. under argon atmosphere, and condensed and refluxed for 48 h. After the mixture was cooled, precipitated, filtered, washed, and dried under vacuum at 80° C. for 12 h to obtain compound 1;
[0081] S2: 8.2 g of compound 1, 4.43 g of dicyandiamide, 0.85 g of potassium hydroxide and 73.8 mL of ethylene glycol methyl ether were added to a container, stirred and mixed evenly, heated in an oil bath at 160°C, and condensed under an argon atmosphere for 24 h. After completion, the mixture was cooled, and formaldehyde was added for ultrasonication. The mixture was first washed with distilled water and then filtered, and then washed with methanol and filtered, and dried under vacuum at 80°C for 48 h to obtain compound 2;
[0082] S3: Add 10.71g of compound 2, 3.28g of terephthalaldehyde and 245mL of dimethyl sulfoxide into a container, evacuate, pass argon, and heat in an oil bath at 180°C. The oil bath heating process adopts a gradient temperature increase, and the temperature is maintained at 50°C, 80°C, 110°C, and 140°C for 5 minutes each. Finally, the temperature is increased to 180°C, condensed and stirred for 48 hours. After the temperature is reached, it is cooled, filtered, extracted with methanol, tetrahydrofuran and dichloromethane for 12 hours each, and dried in a vacuum at 160°C for 24 hours to obtain a composite ultraviolet absorber.
[0083] The present embodiment discloses a polyurethane-acrylate anticorrosive coating, which is composed of the following components in parts by weight: 42 parts of polyurethane, 14 parts of acrylate, 0.11 parts of potassium persulfate, 47 parts of deionized water, 5 parts of modified preservative, and 3.5 parts of composite ultraviolet absorber.
[0084] This embodiment discloses a method for preparing a polyurethane-acrylate anticorrosive coating, comprising the following steps:
[0085] Step (1): first, potassium persulfate is added to deionized water to obtain a potassium persulfate solution, and then the polyurethane is heated in a water bath at 85° C. for 5 min, and then the acrylate and potassium persulfate solution are gradually added dropwise to the polyurethane through a constant pressure funnel, and the dropping time is controlled to be 1 h. After the dropping is completed, the reaction is stirred at 400 rpm for 5 h to obtain a composite emulsion;
[0086] Step (2): Add the modified preservative and the composite UV absorber to the composite emulsion, stir and mix for 2 hours, let stand for 24 hours, and vacuum dry at 60° C. for 18 hours to obtain a polyurethane-acrylate anticorrosive coating.
[0087] Comparative Example 1
[0088] Comparative Example 1 Compared with Example 1, in the preparation process of the modified preservative in Comparative Example 1, benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde is not added, and other conditions remain unchanged.
[0089] Comparative Example 2
[0090] Comparative Example 2 Compared with Example 1, in the preparation process of the modified preservative in Comparative Example 2, 1,3,5-tri(4-aminophenyl)benzene was not added, and other conditions remained unchanged.
[0091] Comparative Example 3
[0092] Comparative Example 3 Compared with Example 1, in the preparation process of the composite ultraviolet absorber in Comparative Example 3, p-aminobenzonitrile was not added, and other conditions remained unchanged.
[0093] Comparative Example 4
[0094] Comparative Example 4 Compared with Example 1, in the preparation process of the composite ultraviolet absorber in Comparative Example 4, no terephthalaldehyde is added, and other conditions remain unchanged.
[0095] Comparative Example 5
[0096] Comparative Example 5 Compared with Example 1, in the preparation process of the polyurethane-acrylate anti-corrosion coating in Comparative Example 5, no modified preservative is added, and other conditions remain unchanged.
[0097] Comparative Example 6
[0098] Compared with Example 1, in Comparative Example 6, during the preparation of the polyurethane-acrylate anti-corrosion coating, no composite ultraviolet absorber was added, and other conditions remained unchanged.
[0099] 1. Corrosion resistance test
[0100] The samples prepared according to Examples 1-5 and Comparative Examples 1-6 were subjected to performance tests. The salt spray resistance of the samples was tested according to GB / T 1771-2007, and the acid and alkali resistance and salt water resistance of the samples were tested according to GB 1763-1979 (1989). The test results are shown in Table 1:
[0101] Table 1
[0102]
[0103] It can be seen from the test results in Table 1 that the polyurethane-acrylate anticorrosive coatings prepared in Examples 1-5 of the present invention have excellent corrosion resistance. By comparing Comparative Example 1 with Examples 1-5, it can be seen that the addition of benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde can make the obtained polyurethane-acrylate anticorrosive coating have excellent corrosion resistance; by comparing Comparative Example 2 with Examples 1-5, it can be seen that the addition of 1,3,5-tris(4-aminophenyl)benzene can make the obtained polyurethane-acrylate anticorrosive coating have excellent corrosion resistance; by comparing Comparative Example 5 with Examples 1-5, it can be seen that the addition of a modified preservative can make the obtained polyurethane-acrylate anticorrosive coating have excellent corrosion resistance.
[0104] 2. Weathering performance test
[0105] The samples prepared according to Examples 1-5 and Comparative Examples 1-6 were subjected to performance tests, and the weather resistance of the samples was tested according to GB / T 1865-2009. The test results are shown in Table 2:
[0106] Table 2
[0107]
[0108] It can be seen from the test results in Table 2 that the polyurethane-acrylate anticorrosive coatings prepared in Examples 1-5 of the present invention have excellent weather resistance. Comparison between Comparative Example 1 and Examples 1-5 shows that the addition of benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde can make the obtained polyurethane-acrylate anticorrosive coating have excellent weather resistance; comparison between Comparative Example 2 and Examples 1-5 shows that the addition of 1,3,5-tri(4-aminophenyl)benzene can make the obtained polyurethane-acrylate anticorrosive coating have excellent weather resistance; comparison between Comparative Example 3 and Examples 1-5 shows that the addition of p-aminobenzonitrile can make the obtained polyurethane The ester-acrylate anti-corrosion coating has excellent weather resistance; from the comparison of Comparative Example 4 and Examples 1-5, it can be seen that the addition of terephthalaldehyde can make the obtained polyurethane-acrylate anti-corrosion coating have excellent weather resistance; from the comparison of Comparative Example 5 and Examples 1-5, it can be seen that the addition of modified preservatives can make the obtained polyurethane-acrylate anti-corrosion coating have excellent weather resistance; from the comparison of Comparative Example 6 and Examples 1-5, it can be seen that the addition of composite UV absorbers can make the obtained polyurethane-acrylate anti-corrosion coating have excellent weather resistance.
[0109] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0110] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. Polyurethane-acrylate anticorrosive coating, characterized in that: The invention is composed of the following components in parts by weight: 30-45 parts of polyurethane, 10-15 parts of acrylate, 0.08-0.12 parts of potassium persulfate, 40-50 parts of deionized water, 3-6 parts of modified preservative, and 2-4 parts of composite ultraviolet absorber, wherein the modified preservative is prepared from benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and 1,3,5-tris(4-aminophenyl)benzene, and the composite ultraviolet absorber is prepared from p-aminobenzonitrile, 4-fluorobenzonitrile, dicyandiamide and terephthalaldehyde; The preparation method of the modified preservative comprises the following steps: Q1: Add benzo[1,2-b:3,4-b':5,6-b']terthiophene-2,5,8-trialdehyde and 1,3,5-tris(4-aminophenyl)benzene to an ampoule, then add 1,3,5-trimethylbenzene, 1,4-dioxane and acetonitrile, mix by ultrasonication, add trifluoroacetic acid, and continue ultrasonication; Q2: After the ultrasonically mixed ampoule is degassed through a freeze-vacuum-thaw cycle, the ampoule is sealed and heated for reaction. After the reaction is completed, the ampoule is opened, washed, soaked, filtered, and vacuum dried to obtain a modified preservative; The preparation method of the composite ultraviolet absorber comprises the following steps: S1: Add p-aminobenzonitrile, N,N-dimethylformamide and cesium fluoride into a container, perform ultrasonic treatment, then add 4-fluorobenzonitrile under stirring, heat under argon atmosphere, condense and reflux, and after completion, cool, precipitate, filter, wash and vacuum dry to obtain compound 1; S2: Add compound 1, dicyandiamide, potassium hydroxide and ethylene glycol methyl ether into a container, stir and mix evenly, heat in an oil bath, and condense under an argon atmosphere. After the reaction is completed, cool, sonicate, filter, and vacuum dry to obtain compound 2; S3: Add compound 2, terephthalaldehyde and dimethyl sulfoxide into a container, evacuate, pass argon, heat in an oil bath, condense and stir, and after completion, cool, filter, extract, and vacuum dry to obtain a composite ultraviolet absorber; In Q1, the usage ratio of benzo[1,2-b:3,4-b':5,6-b']trithiophene-2,5,8-trialdehyde, 1,3,5-tris(4-aminophenyl)benzene, 1,3,5-trimethylbenzene, 1,4-dioxane, acetonitrile and trifluoroacetic acid is (123.9-185.9) mg: (87.86-131.79) mg: (0.6-0.9) mL: (1.2-1.8) mL: (0.025-0.0375) mL: (0.2-0.3) mL, benzo[ The purity of 1,2-b:3,4-b':5,6-b'] trithiophene-2,5,8-trialdehyde is 97%, the purity of 1,3,5-tris(4-aminophenyl)benzene is 98%, the ultrasonic mixing time is 15-25min, and the ultrasonic mixing time is continued for 5-10min; in Q2, the heating reaction temperature is 140-160°C, the reaction time is 70-72h, washing is performed with N,N-dimethylformamide, soaking is performed with formaldehyde, and the vacuum drying temperature is 70-90°C for 20-24h; In S1, the dosage ratio of p-aminobenzonitrile, N,N-dimethylformamide, cesium fluoride and 4-fluorobenzonitrile is (1.18-1.89) g: (50-80) mL: (6.04-9.66) g: (2.66-4.26) g, the heating temperature is 130-150°C, the condensation reflux time is 45-48 h, the vacuum drying temperature is 80-90°C, and the time is 10-12 h; In S2, the amount ratio of compound 1, dicyandiamide, potassium hydroxide and ethylene glycol methyl ether is (5.38-9.14) g: (2.94-4.99) g: (0.55-0.94) g: (50-85) mL, the oil bath heating temperature is 150-160°C, the condensation reaction time is 20-24 h, formaldehyde is added during the ultrasonic process, first washed with distilled water and filtered, then washed with methanol and filtered, the vacuum drying temperature is 80-90°C, and the time is 48-52 h; In the S3, the dosage ratio of compound 2, terephthalaldehyde and dimethyl sulfoxide is (9.96-12.95) g: (2.68-3.48) g: (200-260) mL, the oil bath heating temperature is 180°C, and the condensation stirring time is 48-52 h. The oil bath heating process adopts a gradient temperature increase, and in the process of increasing from room temperature to 50°C, 80°C, 110°C, and 140°C, each is maintained for 5 minutes, and finally the temperature is increased to 180°C, and methanol, tetrahydrofuran and dichloromethane are each extracted for 12 hours. The vacuum drying temperature is 140-160°C and the time is 20-24 hours.
2. The method for preparing the polyurethane-acrylate anticorrosive coating according to claim 1, characterized in that: The following steps are involved: Step (1): firstly, potassium persulfate is added into deionized water to obtain a potassium persulfate solution, then the polyurethane is heated in a water bath, and then the acrylate and the potassium persulfate solution are gradually added dropwise into the polyurethane through a constant pressure funnel, the adding time is controlled, and after the adding is completed, the reaction is stirred to obtain a composite emulsion; Step (2): adding the modified preservative and the composite ultraviolet absorber to the composite emulsion, stirring and mixing, standing, and vacuum drying to obtain a polyurethane-acrylate anticorrosive coating.
3. The method for preparing the polyurethane-acrylate anticorrosive coating according to claim 2, characterized in that: In the step (1), the water bath heating temperature is 80-90°C, the time is 5-8 min, the dripping time is controlled to be 1-1.5 h, the stirring time is 3-5 h, and the stirring speed is 400-600 rpm; in the step (2), the mixing and stirring time is 1-2 h, the standing time is 20-24 h, and the vacuum drying temperature is 50-60°C, and the time is 12-18 h.