Preparation method and application of aircraft cabin adsorbent

By using the metal organic skeleton MOF-303 material with aluminum as the center atom as the aircraft cabin adsorbent, the problem of humidity regulation in the aircraft cabin is solved, and the effective adsorption and humidification functions in low-humidity environments are realized, the humidity control device is simplified, and the humidity control device is reduced. Cost and energy demand.

CN118925689APending Publication Date: 2024-11-12BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192871.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively regulate humidity in the aircraft cabin, especially in low humidity environments, and conventional adsorbents cannot achieve the dual functions of dehumidification and humidification, resulting in complex and high cost of humidity control.

Method used

The metal organic skeleton MOF-303 material with aluminum as the center atom is used as the adsorbent of the aircraft cabin. The material is prepared by hydrothermal method, and its porous structure and high specific surface area are used to effectively absorb moisture in a low humidity environment, and desorption of moisture by heating. To achieve precise humidity control.

Benefits of technology

The effect of stably adjusting humidity in the aircraft cabin is achieved, the energy demand and space limitations of humidity control are reduced, the device design is simplified, the cost is reduced, and the accuracy and stability of humidity control are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925689A_ABST
    Figure CN118925689A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of an aircraft cabin adsorbent, and belongs to the technical field of adsorption material synthesis. The aircraft cabin adsorbent is prepared by stirring, dissolving and reacting 3, 5-pyrazoledicarboxylic acid, alkali and solid aluminum salt in deionized water, and the structure of the aircraft cabin adsorbent is an MOF (Metal Organic Framework) material connected by taking aluminum as a central atom and taking 3, 5-pyrazoledicarboxylic acid as an organic ligand; the surface of the material has a porous structure, large crystals and small particles exist at the same time, the diameter of the large crystals is 2.5-3.5 [mu] m, and the diameter of the small particles is 0.15-0.25 [mu] m; in a normal-temperature environment, when the humidity is lower than 30RH%, the water collecting capacity of the aircraft cabin adsorbent reaches 0.425 g / g, and the water collecting capacity is not obviously reduced along with the increase of the humidity. The method is simple in preparation process, high in yield, stable in water absorption-decomposition effect and wide in application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adsorption material synthesis, and in particular relates to a preparation method and application of an aircraft cabin adsorbent. Background Art

[0002] During a long flight, the humidity in the cabin of an aircraft may decrease or increase due to the difference in humidity in the external environment, which will significantly affect the comfort of the aircraft. Excessive or low humidity will also affect the parameters of the aircraft cabin. In the absence of proper control measures (such as ventilation and adsorbents), moisture accumulation will promote the growth of bacteria, mold and other fungi. Excessive humidity will also affect the structural fatigue and combat readiness of the aircraft. The American Society of Heating, Refrigerating and Air-Conditioning Engineers (ASHRAE) recommends a relative humidity range of 45-65RH%. During the flight of an aircraft, a sudden increase in humidity in the environment can also cause dry eye disease in passengers.

[0003] It is worth noting that in the case of a confined space, it is necessary to maintain a certain humidity level when fresh air is limited or unavailable. Patent CN110697054A discloses a structure of an aircraft cabin humidification system, including a humidifier, a water collection system, a third pipe system, etc. The device is relatively complex and is not conducive to installation and maintenance on the aircraft. Patent CN216332794U discloses an aircraft humidity control device, which also has the disadvantages of complex manufacturing process and high cost. If appropriate adsorbents can be used in the atmospheric environment, the energy requirements and space limitations of the water collection equipment can be greatly reduced. Conventional adsorbents such as zeolite and silica gel usually only control humidity by adsorbing water. This reduction in humidity is irreversible, and when the humidity is too low, it cannot be effectively improved; however, adsorbents that can achieve the dual functions of dehumidification and humidification remain to be explored.

[0004] Recently, metal organic frameworks (MOFs) have been successfully used as adsorbents for collecting and releasing water from the air (Nature Water, 2023, 1, 418–419; Nature Nanotechnology, 2020, 15, 348–355); metal organic frameworks (MOFs) are two-dimensional or three-dimensional porous crystalline materials with highly ordered porous structures, uniform pore size distribution and active sites, making them widely used in gas storage and adsorption, chemical sensing and catalysis. AbdulHalim et al. reported a metal organic framework Y-shp-MOF-5 for indoor humidification and dehumidification (J.Am.Chem.Soc.2017,139,31,10715–10722), but the material has poor water absorption at low humidity, making it difficult to achieve precise humidity control. Summary of the invention

[0005] In view of the problem existing in the humidity regulation of the existing closed space, it is difficult to reduce the humidity when the air humidity is low. The present invention proposes a preparation method and application of an aircraft cabin adsorbent to prepare MOF-303 for regulating the humidity of the aircraft cabin.

[0006] The aircraft cabin adsorbent is MOF-303, which is a MOF material with aluminum as the central atom and 3,5-pyrazoledicarboxylic acid as an organic ligand. The specific surface area of ​​the material reaches 1100m 2 The surface of the material has a porous structure, with large crystals and small particles, and the diameter of the large crystals is 2.5-3.5μm, and the diameter of the small particles is 0.15-0.25μm; in a normal temperature environment, when the humidity is lower than 30RH%, the water collection capacity of the aircraft cabin adsorbent reaches 0.425g / g, and with the increase of humidity, the water collection capacity does not decrease significantly; the aircraft cabin adsorbent has thermal stability within 450°C.

[0007] The preparation method of the aircraft cabin adsorbent comprises the following specific steps:

[0008] Step 1: Add 3,5-pyrazoledicarboxylic acid, a base and a solid aluminum salt into deionized water, and stir until they are completely dissolved to obtain a mixed solution.

[0009] The alkali is one or more of sodium hydroxide, potassium hydroxide, calcium hydroxide, lithium hydroxide and ammonia water; the preferred alkali is sodium hydroxide.

[0010] The aluminum salt is one or more of aluminum chloride hexahydrate, aluminum sulfate 18hydrate, and aluminum potassium sulfate dodecahydrate; the preferred aluminum salt is aluminum chloride hexahydrate.

[0011] The mass ratio of the aluminum salt, 3,5-pyrazoledicarboxylic acid and the base is 3:2:(1-1.5).

[0012] Step 2: react the mixed solution at 60-120° C. for 12-48 hours, stop the reaction, and naturally cool to room temperature to obtain a precipitate.

[0013] The reaction temperature is preferably 100°C.

[0014] The reaction time is preferably 24 h.

[0015] Step 3: Wash, filter and vacuum dry the product after the reaction to obtain solid MOF-303.

[0016] The mixture was washed and filtered twice with N,N-dimethylformamide and methanol respectively. First, N,N-dimethylformamide was used to remove impurities produced after the reaction. Then, methanol was used to replace and remove residual N,N-dimethylformamide, which was beneficial for subsequent vacuum drying.

[0017] The temperature of vacuum drying was 120° C. The vacuum pressure of vacuum drying was −0.1 MPa.

[0018] The yield and ligand conversion rate of MOF-303 prepared by the above method reach over 70% and 80%.

[0019] The specific process of applying aircraft cabin adsorbent MOF-303 to aircraft cabin humidity regulation is as follows:

[0020] In the enclosed space of an aircraft cabin, when the ambient humidity is too high, the aircraft cabin adsorbent collects moisture in the air until the ambient humidity drops to a level suitable for the human body; if it is necessary to continue to reduce the humidity in a low-humidity environment, the adsorption capacity of the aircraft cabin adsorbent can remain stable until the requirement is met; when the humidity in the aircraft cabin is too low, the adsorbent is heated to desorb water molecules, thereby achieving the purpose of increasing the ambient humidity; the above-mentioned water collection and dehydration processes are repeated to achieve the purpose of controlling the ambient humidity of the aircraft cabin.

[0021] The aircraft cabin adsorbent can also be used for humidity control in confined spaces such as space shuttles, cabins, and aircraft manufacturing plants.

[0022] The advantages and positive effects of the present invention are:

[0023] 1. The preparation method of MOF-303 provided by the present invention has simple preparation process, low cost and high yield;

[0024] 2. The MOF-303 prepared by the present invention has uniform size, good stability, and better water absorption and decomposition effect, and can be used as an efficient adsorbent for humidity control materials in aircraft cabins.

[0025] 3. The MOF-303 prepared by the present invention can pave the way for alleviating various existing burdens brought by currently deployed technologies in terms of design capacity, energy efficiency and total cost. The material will serve as a potential adsorbent for humidity control in confined spaces (space shuttles, cabins and aircraft manufacturing plants). BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is an infrared spectrum of MOF-303 prepared in Example 3 of the present invention;

[0027] Figure 2 is the X-ray diffraction pattern of MOF-303 prepared in Example 3 of the present invention;

[0028] Figure 3 is a thermogravimetric analysis diagram of MOF-303 prepared in Example 3 of the present invention;

[0029] Figure 4Graph showing the water absorption capacity of MOF-303 prepared in Example 3 of the present invention in an environment with a temperature of 25° C. and at humidity of 20, 40, and 60 RH% respectively;

[0030] Figure 5 Graphs showing the water absorption capacity of MOF-303 prepared in Example 3 of the present invention at different temperatures in an environment with a humidity of 25 RH%;

[0031] Figure 6 is a graph of water release of MOF-303 prepared in Example 3 of the present invention at different temperatures;

[0032] Figure 7 This is a cycle test diagram of MOF-303 prepared in Example 3 of the present invention at 20 and 60 RH%;

[0033] Figure 8 This is a scanning electron microscope image of MOF-303 prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0034] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments.

[0035] Example 1

[0036] (1) Weigh 0.2 g of 3,5-pyrazoledicarboxylic acid, 0.3 g of aluminum chloride hexahydrate, and 0.1 g of solid sodium hydroxide and dissolve them in 50 mL of deionized water.

[0037] (2) The homogeneous solution formed above was placed in a 100 mL hydrothermal reactor and heated to 100 °C, and grown under this condition for 24 h.

[0038] (3) After growth is complete, turn off the heating device and allow the cells to cool to room temperature.

[0039] (4) Take out the reaction precipitate and place it in a beaker, soak it in DMF for 1 day, filter it and wash it with methanol.

[0040] (5) The obtained precipitated material was separated and then vacuum dried at 120°C to activate the sample to obtain a white powder.

[0041] (6) Determine the MOF-303 yield and ligand conversion rate.

[0042] Example 2

[0043] (1) Weigh 1 g of 3,5-pyrazoledicarboxylic acid, 1.5 g of aluminum chloride hexahydrate, and 0.6 g of solid sodium hydroxide and dissolve them in 250 mL of deionized water.

[0044] (2) The homogeneous solution formed above was placed in a 500 mL hydrothermal reactor and heated to 100° C. and grown under this condition for 24 h.

[0045] (3) After the growth is completed, turn off the addition device and then cool to room temperature.

[0046] (4) Take out the reaction precipitate and place it in a beaker, soak it in DMF for 1 day, filter it and wash it with methanol.

[0047] (5) The obtained precipitated material was separated and then vacuum dried at 120°C to activate the sample to obtain a white powder.

[0048] (6) Determine the MOF-303 yield and ligand conversion rate.

[0049] Example 3

[0050] (1) Weigh 1 g of 3,5-pyrazoledicarboxylic acid, 1.5 g of aluminum chloride hexahydrate, and 0.75 g of solid sodium hydroxide and dissolve them in 250 mL of deionized water.

[0051] (2) The homogeneous solution formed above was placed in a 500 mL hydrothermal reactor and heated to 100° C. and grown under this condition for 24 h.

[0052] (3) After the growth is completed, turn off the addition device and then cool to room temperature.

[0053] (4) Take out the reaction precipitate and place it in a beaker, soak it in DMF for 1 day, filter it and wash it with methanol.

[0054] (5) The obtained precipitated material was separated and then vacuum dried at 120°C to activate the sample to obtain a white powder.

[0055] The obtained white powder was detected by infrared spectrometer and XRD instrument, and the following Figure 1 and Figure 2 The infrared spectrum and XRD diagram shown in the figure show that MOF-303 has a -1 、1477cm -1 and 1525cm -1 The characteristic peaks correspond to the stretching vibrations of N-NH, CC and CN, respectively. From the XRD diagram, it can be seen that the prepared sample has characteristic peaks of MOF-303 at 8.9° and 17.8°, which proves that the preparation of MOF-303 is successful.

[0056] like Figure 3As shown in the figure, it is the thermogravimetric analysis diagram of the prepared white powder, from which it can be seen that the 27.38% weight loss of the prepared MOF-303 at 300°C is attributed to the evaporation of water molecules and the decomposition of non-coordinated H2PZDC. MOF-303 begins to decompose at 457.8°C. At about 540°C, MOF-303 is oxidized to aluminum oxide with a mass loss of 33.13%. The above results show that the prepared MOF-303 has good thermal stability.

[0057] (6) The prepared MOF-303 sample was placed in an environment with a temperature of 25°C and a humidity of 20RH%, 40RH% and 60RH%, and its water absorption curve was tested until the water absorption was saturated. The water collection results are as follows: Figure 4 As shown, it can be seen that the water collection capacity of the prepared MOF-303 sample at 20, 40 and 60 RH% is 0.425, 0.41 and 0.395 g / g respectively; in an environment with a humidity of 25 RH%, at temperatures of 20, 30 and 38.5 ° C, the water absorption capacity of the sample was tested respectively, and the water collection amount was obtained as shown in Figure 5 As shown, it can be seen that the water absorption capacity of MOF-303 at 20, 30 and 38.5 °C is 0.41, 0.375 and 0.348 g / g, respectively.

[0058] (7) The sample that has been saturated with water under the same humidity and temperature conditions is placed in an environment with a humidity of 60 RH% and temperatures of 40°C, 50°C and 60°C to release water and test its water release curve. Figure 6 As shown, it can be seen that MOF-303 released 35%, 45% and 68% of the adsorbed water at 40, 50 and 60 °C, respectively.

[0059] (8) Figure 8 As shown, the surface of the prepared sample has a porous structure, with large crystals and small particles coexisting, and the diameter of the large crystals is 2.5-3.5 μm, and the diameter of the small particles is 0.15-0.25 μm.

[0060] (9) About 300 mg of the prepared sample was placed in a 15*15 cm acrylic device, and the humidity was controlled at 60% and 25% respectively. After two hours of saturation adsorption, the sample was taken out and the water collection capacity of MOF-303 was calculated. After the water absorption was completed, the sample was placed in an oven at 80°C to desorb water molecules. Then the test was repeated 10 times in sequence, and the water collection capacity was compared. Figure 7 As shown, in different humidity environments, the water collection amount of the samples prepared by the present invention is slightly different, which proves that the samples prepared by the present invention can achieve good water absorption effect in normal humidity and low humidity environments; after the cycle test, the water collection amount did not show a significant decrease, indicating that the samples prepared by the present invention have good stability.

[0061] Example 4

[0062] (1) Weigh 1 g of 3,5-pyrazoledicarboxylic acid, 1.5 g of aluminum chloride hexahydrate, and 0.75 g of solid sodium hydroxide and dissolve them in 250 mL of deionized water.

[0063] (2) The homogeneous solution formed above was placed in a 500 mL hydrothermal reactor and heated to 100° C., and grown under this condition for 12 h.

[0064] (3) After the growth is completed, turn off the addition device and then cool to room temperature.

[0065] (4) Take out the reaction precipitate and place it in a beaker, soak it in DMF for 1 day, filter it and wash it with methanol.

[0066] (5) The obtained precipitated material was separated and then vacuum dried at 120°C to activate the sample to obtain a white powder.

[0067] (6) Determine the MOF-303 yield and ligand conversion rate.

[0068] Example 5

[0069] (1) Weigh 1 g of 3,5-pyrazoledicarboxylic acid, 1.5 g of aluminum chloride hexahydrate, and 0.75 g of solid sodium hydroxide and dissolve them in 250 mL of deionized water.

[0070] (2) The homogeneous solution formed above was placed in a 500 mL hydrothermal reactor and heated to 100° C., and grown under this condition for 48 h.

[0071] (3) After the growth is completed, turn off the addition device and then cool to room temperature.

[0072] (4) Take out the reaction precipitate and place it in a beaker, soak it in DMF for 1 day, filter it and wash it with methanol.

[0073] (5) The obtained precipitated material was separated and then vacuum dried at 120°C to activate the sample to obtain a white powder.

[0074] (6) Determine the MOF-303 yield and ligand conversion rate.

[0075] Example 6

[0076] (1) Weigh 1 g of 3,5-pyrazoledicarboxylic acid, 1.5 g of aluminum chloride hexahydrate, and 0.75 g of solid sodium hydroxide and dissolve them in 250 mL of deionized water.

[0077] (2) The homogeneous solution formed above was placed in a 500 mL hydrothermal reactor and heated to 120°C. The cells were grown under this condition for 12 h.

[0078] (3) After the growth is completed, turn off the addition device and then cool to room temperature.

[0079] (4) Take out the reaction precipitate and place it in a beaker, soak it in DMF for 1 day, filter it and wash it with methanol.

[0080] (5) The obtained precipitated material was separated and then vacuum dried at 120°C to activate the sample to obtain a white powder.

[0081] (6) Determine the MOF-303 yield and ligand conversion rate.

[0082] Example 7

[0083] (1) Weigh 1 g of 3,5-pyrazoledicarboxylic acid, 1.5 g of aluminum chloride hexahydrate, and 0.75 g of solid sodium hydroxide and dissolve them in 250 mL of deionized water.

[0084] (2) The homogeneous solution formed above was placed in a 500 mL hydrothermal reactor and heated to 120°C, and grown under this condition for 24 hours.

[0085] (3) After the growth is completed, turn off the addition device and then cool to room temperature.

[0086] (4) Take out the reaction precipitate and place it in a beaker, soak it in DMF for 1 day, filter it and wash it with methanol.

[0087] (5) The obtained precipitated material was separated and then vacuum dried at 120°C to activate the sample to obtain a white powder.

[0088] (6) Determine the MOF-303 yield and ligand conversion rate.

[0089] Example 8

[0090] (1) Weigh 1 g of 3,5-pyrazoledicarboxylic acid, 1.5 g of aluminum chloride hexahydrate, and 0.75 g of solid sodium hydroxide and dissolve them in 250 mL of deionized water.

[0091] (2) The homogeneous solution formed above was placed in a 500 mL hydrothermal reactor and heated to 120° C. and grown under this condition for 48 h.

[0092] (3) After the growth is completed, turn off the addition device and then cool to room temperature.

[0093] (4) Take out the reaction precipitate and place it in a beaker, soak it in DMF for 1 day, filter it and wash it with methanol.

[0094] (5) The obtained precipitated material was separated and then vacuum dried at 120°C to activate the sample to obtain a white powder.

[0095] (6) Determine the MOF-303 yield and ligand conversion rate.

[0096] Table 1 shows the yields of MOF-303 and ligand conversion rates in Examples 1 to 8 above, wherein the reaction yield and ligand conversion rate of Example 3 can reach 77.2% and 85.6%, respectively.

[0097] Table 1 Yield and conversion rate of MOF-303 prepared in Examples 1-8

[0098]

Claims

1. An aircraft cabin adsorbent, It is characterized in that MOF-303 is a MOF material with aluminum as the central atom and 3,5-pyrazoledicarboxylic acid as the organic ligand. The specific surface area of ​​this material reaches 1100m 2 The surface of the material has a porous structure, with large crystals and small particles. The diameter of the large crystals is 2.5-3.5μm, and the diameter of the small particles is 0.15-0.25μm. In a normal temperature environment, when the humidity is lower than 30RH%, the water collection capacity of the aircraft cabin adsorbent reaches 0.425g / g, and with the increase of humidity, the water collection capacity does not decrease significantly.

2. An aircraft cabin adsorbent, It is characterized in that The aircraft cabin adsorbent has thermal stability within 450°C.

3. A method for preparing an aircraft cabin adsorbent, It is characterized in that The specific steps are as follows: Step 1, adding 3,5-pyrazoledicarboxylic acid, a base and a solid aluminum salt into deionized water, stirring until completely dissolved, to obtain a mixed solution; The mass ratio of the aluminum salt, 3,5-pyrazoledicarboxylic acid and the base is 3:2:(1-1.5); Step 2, reacting the mixed solution at 60-120° C. for 12-48 hours, stopping the reaction and naturally cooling to room temperature to obtain a precipitate; Step 3, washing, filtering and vacuum drying the product after the reaction to obtain solid MOF-303; The mixture was washed and filtered twice with N,N-dimethylformamide and methanol respectively. First, N,N-dimethylformamide was used to remove impurities produced after the reaction. Then, methanol was used to replace and remove residual N,N-dimethylformamide, which was beneficial for subsequent vacuum drying.

4. The preparation method according to claim 3, It is characterized in that The alkali is one or two or more of sodium hydroxide, potassium hydroxide, calcium hydroxide, lithium hydroxide and ammonia water.

5. The preparation method according to claim 4, It is characterized in that The base is preferably sodium hydroxide.

6. The preparation method according to claim 3, It is characterized in that The aluminum salt is one or two or more of aluminum chloride hexahydrate, aluminum sulfate 18hydrate and aluminum potassium sulfate dodecahydrate.

7. The preparation method according to claim 6, It is characterized in that The aluminum salt is preferably aluminum chloride hexahydrate.

8. The preparation method according to claim 3, It is characterized in that The yield of solid MOF-303 is over 70%, and the ligand conversion rate is over 80%.

9. An application method of an aircraft cabin adsorbent, It is characterized in that The specific process of regulating aircraft cabin humidity is: In the enclosed space of an aircraft cabin, when the ambient humidity is too high, the aircraft cabin adsorbent collects moisture in the air until the ambient humidity drops to a level suitable for the human body; if it is necessary to continue to reduce the humidity in a low-humidity environment, the adsorption capacity of the aircraft cabin adsorbent can remain stable until the requirement is met; when the humidity in the aircraft cabin is too low, the adsorbent is heated to desorb water molecules, thereby achieving the purpose of increasing the ambient humidity; the above-mentioned water collection and dehydration processes are repeated to achieve the purpose of controlling the ambient humidity of the aircraft cabin.

10. The method for using the aircraft cabin adsorbent according to claim 9, It is characterized in that It can also be used for humidity control in confined spaces of space shuttles, cabins and aircraft manufacturing plants.