Method for recovering iron and aluminum and recovering acid through acid leaching of red mud

Through strong acid and acid leaching method and a series of process steps, the efficient recycling of iron aluminum and acid recovery problems in red mud are solved, and the resource utilization of low-cost and low-pollution is achieved, the subsequent alkali consumption and environmental pollution are reduced, and the red is improved. Comprehensive utilization rate of mud.

CN118957269AActive Publication Date: 2024-11-15SHANDONG XILI ENVIRONMENTAL TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411033064.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The high alkalinity of red mud leads to the acid leaching method that consumes acid and alkaline when recycling valuable metal elements, and the product contains a large amount of residual acid liquid, resulting in secondary pollution. The comprehensive utilization rate of red mud is low and the environment is present. Pollution and waste of resources.

Method used

Using strong acid and acid leaching method, and through a series of stirring, heating and evaporation and pH adjustment steps, the recovery of iron and aluminum and strong acids can be achieved, acid and alkali consumption are reduced, waste slag and sewage discharge are reduced, and high-purity iron and aluminum hydroxides are generated. and sodium metaaluminate to promote resource utilization.

Benefits of technology

With low acid consumption and low alkali consumption, efficient recycling of iron and aluminum in red mud is achieved, strong acid is recovered, and subsequent alkali consumption is reduced. The obtained product contains less impurities, which is convenient for subsequent resource utilization and reduced treatment Cost and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957269A_ABST
    Figure CN118957269A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of solid resource utilization, and relates to a method for recovering iron and aluminum and recovering acid by red mud acid leaching, which comprises the following steps: (1) leaching red mud with strong acid to obtain red mud slag and an iron and aluminum solution; (2) mixing the red mud slag with desalted water to obtain acid radical-removed red mud slag and a sodium salt solution; (3) stirring, heating and evaporating the iron-aluminum solution to obtain an iron-aluminum mixed solid and a recycled strong acid solution; (4) adjusting the pH value of the iron-aluminum mixed solid to obtain an iron-aluminum hydroxide solid and a sodium salt solution; (5) mixing the iron-aluminum mixed solid with desalted water to obtain an acid radical-removed iron-aluminum mixed solid and a sodium salt solution; and (6) adjusting the pH value of the acid radical removed iron-aluminum mixed solid to obtain a ferric hydroxide solid and a sodium metaaluminate solution. According to the method, the recovery of iron and aluminum in the red mud is realized under the condition of low acid consumption and low alkali consumption; strong acid is recycled on the basis of recycling iron and aluminum, and energy consumption for recycling the strong acid is small; and the obtained red mud slag, ferric hydroxide and sodium metaaluminate solution contain few impurities, so that the subsequent process is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid resource utilization and relates to a method for recovering iron and aluminum and acid by acid leaching of red mud. Background Art

[0002] Red mud is a strong alkaline byproduct discharged during the production of alumina. It is a typical bulk solid waste of the non-ferrous metallurgical industry. Metallic aluminum is mainly extracted from alumina. One ton of electrolytic aluminum requires about 2 tons of alumina, and the production of one ton of alumina requires 2 to 3 tons of bauxite, and a large amount of red mud is produced in this process. According to statistics, my country's annual red mud production has exceeded 100 million tons since 2017. However, the comprehensive utilization rate of red mud in my country is less than 10%. The accumulation treatment not only occupies land but also pollutes the surrounding environment, and there is a risk of dam breach, which poses a serious threat to ecological security.

[0003] Red mud contains a large amount of valuable components such as iron oxide and aluminum oxide. The proportion of iron and aluminum exceeds 50%, making it a good raw material for extracting iron and aluminum. At present, there have been many studies on the recovery of valuable metal elements in red mud. Acid leaching is a relatively simple method for recovering valuable elements in red mud. Commonly used acids include organic acids, such as oxalic acid, citric acid, etc., and inorganic acids, such as hydrochloric acid, nitric acid, sulfuric acid, etc. Due to the high alkalinity of red mud, the acid leaching method often consumes too much acid and alkali, and the obtained product contains a large amount of residual acid, resulting in secondary pollution.

[0004] Therefore, how to develop a sustainable bulk solid waste treatment technology that combines waste reduction and resource recovery, and how to reduce acid and alkali consumption or recycle the used acid to achieve high-purity products is an effective way to practice a circular economy and promote sustainable development, and has positive significance in solving environmental pollution problems. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a method for recovering iron and aluminum and recovering acid by acid leaching of red mud, thereby achieving harmlessness and resource utilization of red mud and recovery of strong acid. The specific technical scheme is as follows:

[0006] A method for recovering iron, aluminum and acid by acid leaching of red mud comprises the following steps:

[0007] (1) crushing the red mud and mixing it with a strong acid solution, stirring it continuously under heating conditions to leach out the iron and aluminum solution, and obtaining red mud residue and the iron and aluminum solution after solid-liquid separation;

[0008] (2) mixing the red mud residue obtained in step (1) with desalted water, stirring and separating the solid and liquid to obtain the acid-free red mud residue and sodium salt solution;

[0009] (3) stirring, heating and evaporating the iron-aluminum solution obtained in step (1) to obtain an iron-aluminum mixed solid and gas, collecting the generated gas and vacuum cooling to obtain a strong acid solution;

[0010] (4) mixing the iron-aluminum mixed solid obtained in step (3) with a NaOH solution, adjusting the pH to 5 to 6, stirring and separating the solid and the liquid to obtain an iron-aluminum hydroxide solid and a sodium salt solution;

[0011] (5) mixing the iron aluminum hydroxide solid obtained in step (4) with desalted water, stirring and separating the solid and the liquid to obtain the iron aluminum hydroxide solid with the acid radical removed and the sodium salt solution;

[0012] (6) The deacidified iron aluminum hydroxide solid obtained in step (5) is mixed with a NaOH solution, the pH value is adjusted to 10 to 14, and the solid-liquid separation is performed after stirring to obtain an iron hydroxide solid and a sodium aluminate solution.

[0013] Furthermore, in step (1), the red mud includes Bayer process red mud, sintering process red mud or combined process red mud.

[0014] Furthermore, the red mud is crushed into a particle size of 60 to 200 meshes.

[0015] Furthermore, in the step (1), the mass concentration of the strong acid is 15% to 36%; the iron-aluminum solution is leached in a cycle for 3 to 6 times, and the iron-aluminum solution is leached in a cycle, which means that red mud and the strong acid solution are heated and stirred, solid-liquid separation is performed, and red mud residue and iron-aluminum solution are obtained; the red mud residue is heated and stirred with the strong acid solution, solid-liquid separation is performed, and red mud residue and iron-aluminum solution are obtained; the mass volume ratio of the red mud or red mud residue to the strong acid solution is 1kg: (1L to 5L) each time, the stirring time is 30min to 12h, and the stirring temperature is 50 to 95°C, and finally red mud residue and a mixed iron-aluminum solution are obtained.

[0016] Furthermore, the step (1) specifically includes (1-1) mixing red mud with a strong acid having a mass concentration of 31%, placing the mixture in a water constant temperature oscillator at 80°C for reaction for 30 minutes, wherein the mass volume ratio of the red mud to the strong acid is 1kg:1L, and filtering after the reaction to obtain red mud residue and an iron-aluminum solution; (1-2) mixing the red mud residue with a strong acid having a mass concentration of 20%, placing the mixture in a water constant temperature oscillator at 90°C for reaction for 30 minutes, wherein the mass volume ratio of the red mud to the strong acid is 1kg:1L, and filtering after the reaction to obtain red mud residue and an iron-aluminum solution; (1-3) performing step (1-2) twice on the red mud residue obtained each time; and (1-4) combining all the iron-aluminum solutions.

[0017] Furthermore, the strong acid is an organic acid or an inorganic acid; the organic acid is oxalic acid or citric acid, and the inorganic acid is hydrochloric acid, nitric acid or sulfuric acid.

[0018] Furthermore, in the step (2), the mass volume ratio of red mud slag to desalted water is 1 kg: (500 mL-5 L); in the step (3), the heating and evaporation methods include steam heating, electric heating and coal heating, and the heating and evaporation temperature is 100-200° C.; the gas cooling methods include natural cooling and condensed water cooling.

[0019] Furthermore, in step (4), the stirring time is 15 min to 6 h.

[0020] Furthermore, in step (5), the mass volume ratio of the iron-aluminum mixed solid to the desalted water is 1 kg: (500 mL-5 L).

[0021] Furthermore, in step (6), the stirring time is 15 min to 6 h.

[0022] The beneficial effects of the present invention are as follows:

[0023] (1) The present invention adopts a strong acid leaching and enrichment and concentration process to achieve the recovery of iron and aluminum in red mud under the condition of low acid consumption and low alkali consumption; the treatment process is simple, the cost is reduced, and there is no discharge of waste residue and sewage.

[0024] (2) In addition to recovering iron and aluminum, the present invention also recovers strong acid, and promotes the hydrolysis of iron and aluminum during evaporation to generate Fe(OH)3 and Al(OH)3, thereby reducing subsequent alkali consumption, and the energy consumption in the process of recovering strong acid is relatively small.

[0025] (3) The red mud residue, ferric hydroxide and sodium aluminate solution obtained by the present invention contain less impurities, especially less acid ions, which is convenient for the subsequent resource utilization of the red mud residue and the use of sodium aluminate in the electrolytic aluminum process. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a process flow chart of the method for recovering iron and aluminum and recovering acid by acid leaching of red mud according to the present invention;

[0027] Figure 2 is a photograph of the original red mud used in Example 1;

[0028] Figure 3 This is a photo of the red mud residue obtained in step (2) of Example 1;

[0029] Figure 4 The SEM and EDS images of the red mud residue obtained in step (2) of Example 1;

[0030] Figure 5 The XRD diagram of the red mud used in Example 1 and the red mud residue obtained in step (2);

[0031] Figure 6is a photograph of the iron hydroxide solid obtained in Example 1;

[0032] Figure 7 This is a photograph of the sodium aluminate solution obtained in Example 1. DETAILED DESCRIPTION

[0033] The instruments, reagents, materials, etc. involved in the following embodiments, unless otherwise specified, are all conventional instruments, reagents, materials, etc. in the prior art and can be obtained through regular commercial channels. The experimental methods, detection methods, etc. involved in the following embodiments, unless otherwise specified, are all conventional experimental methods, detection methods, etc. in the prior art.

[0034] In the following examples and comparative examples of the present invention, the red mud used is from the Bayer red mud of Shandong Xinfa Group, and the percentage contents of iron and aluminum are 20.29% and 9.67% respectively; the particle size of the red mud after crushing is 60-200 mesh. The main raw materials, strong acid and sodium hydroxide, come from an electrolytic aluminum plant.

[0035] Example 1

[0036] like Figure 1 As shown, a method for recovering iron and aluminum and recovering acid by acid leaching of red mud comprises the following steps:

[0037] (1) After crushing, the red mud is mixed with a strong acid solution with a mass concentration of 31%, and placed in a water constant temperature oscillator at 80° C. for reaction for 2 hours. The mass volume ratio of the red mud to the strong acid is 1 kg:5 L. After the reaction, red mud residue and iron-aluminum solution are obtained by filtration; the Bayer process red mud is leached with a high concentration of strong acid, so that Fe and Al in the red mud enter the leaching solution as much as possible;

[0038] (2) mixing the red mud residue obtained in step (1) with desalted water in a mass volume ratio of 1 kg:1 L, stirring for 30 min to separate the solid and liquid, and obtaining the acid-free red mud residue and sodium salt solution;

[0039] (3) placing the iron-aluminum solution obtained in step (1) in a heating mantle at 180° C. and stirring, heating and evaporating to obtain an iron-aluminum mixed solid and gas, collecting the generated gas and evacuating it using a vacuum pump, and cooling it using cooling water at 20° C. to obtain a strong acid solution;

[0040] (4) mixing the iron-aluminum mixed solid obtained in step (3) with a NaOH solution having a concentration of 130 mg / L, adjusting the pH to 5.5, stirring for 30 min, and separating the solid and the liquid to obtain an iron-aluminum hydroxide solid and a sodium salt solution;

[0041] (5) mixing the iron aluminum hydroxide solid obtained in step (4) with desalted water, wherein the mass volume ratio of the iron aluminum hydroxide solid to the desalted water is 1 kg:1 L, stirring for 30 minutes to separate the solid and the liquid, and obtaining the iron aluminum hydroxide solid without acid radicals and a sodium salt solution;

[0042] (6) The deacidified iron aluminum hydroxide solid obtained in step (5) was mixed with a NaOH solution having a concentration of 130 mg / L, the pH was adjusted to 13, and the solid-liquid separation was performed after stirring for 30 minutes to obtain an iron hydroxide solid and a sodium aluminate solution.

[0043] The photo of the red mud residue obtained in step (1) of this embodiment is as follows Figure 3 As shown, compared with the original red mud (such as Figure 2 Compared with the red mud residue obtained in step (2), the red mud residue is gray in color, indicating that the iron is leached and recovered; the red mud residue obtained in step (2) is digested to test the iron and aluminum content, and the recovery rate of iron and aluminum is obtained. The results are shown in Table 1; SEM and EDS tests are performed on the red mud and red mud residue, respectively, and the results are as follows Figure 4 As shown in Figure 2, the color of iron and aluminum becomes significantly lighter, indicating that iron and aluminum are leached and recovered; the XRD diagrams of the red mud and red mud residue used are shown in Figure 2. Figure 5 As shown; the mass concentration of the strong acid solution obtained in step (3) of the test, the results are shown in Table 1, and the mass concentration of the recovered strong acid solution can reach 12.86%; the volume of NaOH consumed in step (5), the results are shown in Table 1; the digital photo of the iron hydroxide solid obtained in step (6) is shown Figure 6 As shown, it is a red powder, and the obtained sodium aluminate solution is as follows Figure 7 shown.

[0044] Example 2

[0045] A method for recovering iron, aluminum and acid by acid leaching of red mud comprises the following steps:

[0046] (1) After crushing, the red mud is mixed with a strong acid solution with a mass concentration of 20%, placed in a water constant temperature oscillator at 80°C for 2 hours, and the mass volume ratio of the red mud to the strong acid is 1kg:5L. After the reaction, red mud residue and iron-aluminum solution are obtained by filtration;

[0047] (2) mixing the red mud residue obtained in step (1) with desalted water in a mass volume ratio of 1 kg:1 L, stirring for 30 min to separate the solid and liquid, and obtaining the acid-free red mud residue and sodium salt solution;

[0048] (3) placing the iron-aluminum solution obtained in step (1) in a heating mantle at 180° C. and stirring, heating and evaporating to obtain an iron-aluminum mixed solid and gas, collecting the generated gas and evacuating it using a vacuum pump, and cooling it using cooling water at 20° C. to obtain a strong acid solution;

[0049] (4) mixing the iron-aluminum mixed solid obtained in step (3) with a NaOH solution having a concentration of 130 mg / L, adjusting the pH to 5.5, stirring for 30 min, and separating the solid and the liquid to obtain an iron-aluminum hydroxide solid and a sodium salt solution;

[0050] (5) mixing the iron aluminum hydroxide solid obtained in step (4) with desalted water, wherein the mass volume ratio of the iron aluminum hydroxide solid to the desalted water is 1 kg:1 L, stirring for 30 minutes to separate the solid and the liquid, and obtaining the iron aluminum hydroxide solid without acid radicals and a sodium salt solution;

[0051] (6) The deacidified iron aluminum hydroxide solid obtained in step (5) was mixed with a NaOH solution having a concentration of 130 mg / L, the pH was adjusted to 13, and the solid-liquid separation was performed after stirring for 30 minutes to obtain an iron hydroxide solid and a sodium aluminate solution.

[0052] In this embodiment, the red mud residue obtained in step (2) was digested and tested for the iron and aluminum content to obtain the iron and aluminum recovery rate, and the results are shown in Table 1; the mass concentration of the strong acid solution obtained in step (3) was tested, and the results are shown in Table 1. The mass concentration of the recovered strong acid solution can reach 5.78%; the volume of NaOH consumed in step (4) is shown in Table 1.

[0053] Example 3

[0054] A method for recovering iron, aluminum and acid by acid leaching of red mud comprises the following steps:

[0055] (1) Separating red mud residue and iron-aluminum solution; specifically comprising (1-1) mixing red mud with a strong acid having a mass concentration of 31%, placing the mixture in a water constant temperature oscillator at 80°C for reaction for 30 minutes, wherein the mass volume ratio of red mud to strong acid is 1kg:1L, and filtering after the reaction to obtain red mud residue and iron-aluminum solution; (1-2) mixing red mud residue with a strong acid having a mass concentration of 20%, placing the mixture in a water constant temperature oscillator at 90°C for reaction for 30 minutes, wherein the mass volume ratio of red mud to strong acid is 1kg:1L, and filtering after the reaction to obtain red mud residue and iron-aluminum solution; (1-3) performing step (1-2) twice on the red mud residue obtained each time; and (1-4) combining all iron-aluminum solutions.

[0056] (2) mixing the red mud residue obtained in step (1) with desalted water in a mass volume ratio of 1 kg:1 L, stirring for 30 min to separate the solid and liquid, and obtaining the acid-free red mud residue and sodium salt solution;

[0057] (3) placing the iron-aluminum solution obtained in step (1) in a heating mantle at 180° C. and stirring, heating and evaporating to obtain an iron-aluminum mixed solid and gas, collecting the generated gas and evacuating it using a vacuum pump, and cooling it using cooling water at 20° C. to obtain a strong acid solution;

[0058] (4) mixing the iron-aluminum mixed solid obtained in step (3) with a NaOH solution having a concentration of 130 mg / L, adjusting the pH to 5.5, stirring for 30 min, and separating the solid and the liquid to obtain an iron-aluminum hydroxide solid and a sodium salt solution;

[0059] (5) mixing the iron aluminum hydroxide solid obtained in step (4) with desalted water, wherein the mass volume ratio of the iron aluminum hydroxide solid to the desalted water is 1 kg:1 L, stirring for 30 minutes to separate the solid and the liquid, and obtaining the iron aluminum hydroxide solid without acid radicals and a sodium salt solution;

[0060] (6) The deacidified iron aluminum hydroxide solid obtained in step (5) was mixed with a NaOH solution having a concentration of 130 mg / L, the pH was adjusted to 13, and the solid-liquid separation was performed after stirring for 30 minutes to obtain an iron hydroxide solid and a sodium aluminate solution.

[0061] In this embodiment, the red mud residue obtained in step (2) was digested and tested for the iron and aluminum content to obtain the recovery rate of iron and aluminum. The results are shown in Table 1. The mass concentration of the strong acid solution obtained in step (3) was tested. The results are shown in Table 1. The mass concentration of the recovered strong acid solution can reach 6.08%; the volume of NaOH consumed in step (4) is shown in Table 1.

[0062] In the above embodiments, hydrochloric acid is used as the strong acid. Therefore, step (2) obtains the chlorine-free red mud residue and sodium chloride solution; step (4) obtains the iron-aluminum hydroxide solid and sodium chloride solution; step (5) obtains the chlorine-free iron-aluminum hydroxide solid and sodium chloride solution.

[0063] Comparative Example 1

[0064] (1) The crushed red mud was mixed with a hydrochloric acid solution with a mass concentration of 31%, and placed in a water constant temperature oscillator at 80°C for 2 hours. The mass volume ratio of the red mud to the strong acid was 1 kg: 5 L. After the reaction, red mud residue and iron-aluminum solution were obtained by suction filtration. The strong acid used was hydrochloric acid.

[0065] (2) mixing the red mud residue obtained in step (1) with desalted water in a mass volume ratio of 1 kg:1 L, stirring for 30 min to separate the solid and liquid, and obtaining a dechlorinated red mud residue and a sodium chloride solution;

[0066] (3) mixing the iron-aluminum solution obtained in step (1) with a NaOH solution having a concentration of 130 mg / L, adjusting the pH to 5.5, stirring for 30 min, and performing solid-liquid separation to obtain an iron-aluminum hydroxide solid and a sodium chloride solution;

[0067] (4) mixing the iron aluminum hydroxide solid obtained in step (3) with desalted water, wherein the mass volume ratio of the iron aluminum hydroxide solid to the desalted water is 1 kg:1 L, stirring for 30 minutes to separate the solid and the liquid, and obtaining the chlorine-free iron aluminum hydroxide solid and the sodium chloride solution;

[0068] (5) The deacidified iron aluminum hydroxide solid obtained in step (4) was mixed with a NaOH solution having a concentration of 130 mg / L, the pH was adjusted to 13, and the solid-liquid separation was performed after stirring for 30 minutes to obtain an iron hydroxide solid and a sodium aluminate solution.

[0069] In this comparative example, the red mud residue obtained in step (2) was digested to test the iron and aluminum contents, and the recovery rate of iron and aluminum was obtained. The results are shown in Table 1; the volume of NaOH consumed in step (3) is also shown in Table 1.

[0070] Table 1 Data related to Examples 1-3 and Comparative Example 1

[0071]

[0072] It can be seen from the results in Table 1 that the method for recovering iron and aluminum and recovering acid by acid leaching of red mud of the present invention has a high recovery rate of Fe and Al, providing a feasible solution for the resource utilization of red mud; and by recovering the strong acid, the alkali consumption is greatly reduced, and the recovered strong acid also has a high concentration and a high utilization value; the sodium aluminate (solution) and sodium salt (solution) in the product can also be reused in the electrolytic aluminum plant to realize the economic treatment of red mud.

[0073] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for recovering iron, aluminum and acid by acid leaching of red mud, characterized in that: The following steps are involved: (1) crushing the red mud and mixing it with a strong acid solution, stirring it continuously under heating conditions to leach out the iron and aluminum solution, and obtaining red mud residue and the iron and aluminum solution after solid-liquid separation; (2) mixing the red mud residue obtained in step (1) with desalted water, stirring and separating the solid and liquid to obtain the acid-free red mud residue and sodium salt solution; (3) stirring, heating and evaporating the iron-aluminum solution obtained in step (1) to obtain an iron-aluminum mixed solid and gas, collecting the generated gas and vacuum cooling to obtain a strong acid solution; (4) mixing the iron-aluminum mixed solid obtained in step (3) with a NaOH solution, adjusting the pH to 5 to 6, stirring and separating the solid and the liquid to obtain an iron-aluminum hydroxide solid and a sodium salt solution; (5) mixing the iron aluminum hydroxide solid obtained in step (4) with desalted water, stirring and separating the solid and the liquid to obtain the iron aluminum hydroxide solid with the acid radical removed and the sodium salt solution; (6) The deacidified iron aluminum hydroxide solid obtained in step (5) is mixed with a NaOH solution, the pH value is adjusted to 10 to 14, and the solid-liquid separation is performed after stirring to obtain an iron hydroxide solid and a sodium aluminate solution.

2. The method for recovering iron, aluminum and acid by acid leaching of red mud according to claim 1, characterized in that: In the step (1), the red mud includes Bayer process red mud, sintering process red mud or combined process red mud.

3. The method for recovering iron, aluminum and acid by acid leaching of red mud according to claim 1, characterized in that: The red mud is crushed into particles of 60 to 200 meshes.

4. The method for recovering iron, aluminum and acid by acid leaching of red mud according to claim 1, characterized in that: In the step (1), the mass concentration of the strong acid is 15% to 36%; the iron-aluminum solution is leached in a cycle for 3 to 6 times, and the iron-aluminum solution is leached in a cycle, which means that red mud and a strong acid solution are heated and stirred, solid-liquid separation is performed, and red mud residue and an iron-aluminum solution are obtained; the red mud residue is heated and stirred with a strong acid solution, solid-liquid separation is performed, and red mud residue and an iron-aluminum solution are obtained; the mass volume ratio of the red mud or red mud residue to the strong acid solution is 1kg: (1L to 5L) each time, the stirring time is 30min to 12h, and the stirring temperature is 50 to 95°C, and finally red mud residue and a mixed iron-aluminum solution are obtained.

5. The method for recovering iron, aluminum and acid by acid leaching of red mud according to claim 1, characterized in that: The step (1) specifically includes (1-1) mixing red mud with a strong acid having a mass concentration of 31%, placing the mixture in a water constant temperature oscillator at 80°C for reaction for 30 minutes, wherein the mass volume ratio of the red mud to the strong acid is 1kg:1L, and filtering after the reaction to obtain red mud residue and an iron-aluminum solution; (1-2) mixing the red mud residue with a strong acid having a mass concentration of 20%, placing the mixture in a water constant temperature oscillator at 90°C for reaction for 30 minutes, wherein the mass volume ratio of the red mud to the strong acid is 1kg:1L, and filtering after the reaction to obtain red mud residue and an iron-aluminum solution; (1-3) performing step (1-2) twice on the red mud residue obtained each time; and (1-4) combining all the iron-aluminum solutions.

6. The method for recovering iron, aluminum and acid by acid leaching of red mud according to claim 1, characterized in that: The strong acid is an organic acid or an inorganic acid; the organic acid is oxalic acid or citric acid, and the inorganic acid is hydrochloric acid, nitric acid or sulfuric acid.

7. The method for recovering iron, aluminum and acid by acid leaching of red mud according to claim 1, characterized in that: In the step (2), the mass volume ratio of red mud slag to desalted water is 1 kg: (500 mL-5 L); in the step (3), the heating and evaporation methods include steam heating, electric heating and coal heating, and the heating and evaporation temperature is 100-200° C.; the gas cooling methods include natural cooling and condensed water cooling.

8. The method for recovering iron, aluminum and acid by acid leaching of red mud according to claim 1, characterized in that: In the step (4), the stirring time is 15 min to 6 h.

9. The method for recovering iron, aluminum and acid by acid leaching of red mud according to claim 1, characterized in that: In the step (5), the mass volume ratio of the iron-aluminum mixed solid to the desalted water is 1 kg: (500 mL-5 L).

10. The method for recovering iron, aluminum and acid by acid leaching of red mud according to claim 1, characterized in that: In the step (6), the stirring time is 15 min to 6 h.

Citation Information

Patent Citations

  • Method for separating iron and aluminum in red mud

    CN114752774A

  • Red mud resource utilization method

    CN116177554A

  • Method for recovering iron and aluminum from red mud

    CN116516156A

  • Method for recovering nickel from iron-aluminum slag obtained by battery powder leaching

    GB202318269D0

  • Process for treating red mud to recover metal values therefrom

    US6248302B1