Catalytic oxidation method for removing volatile organic compounds by utilizing electric field
By loading active ingredients on the silicon carbide substrate and using the action of electric fields, efficient catalytic oxidation of volatile organic compounds at low temperatures is achieved, and the problems of low temperature efficiency and high cost of precious metals in the existing technology are solved, and the amount of catalyst is reduced, and new VOCs emission control method.
Patent Information
- Application Number
- CN202411112176.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to efficiently remove low-concentration volatile organic compounds in natural gas engine exhaust, industrial fixed source flue gas and catering oil fume under low temperature conditions, especially methane, propane, benzene, etc., and precious metal catalysts are costly and have low efficiency, making them difficult to achieve great Scale application.
Using silicon carbide substrate catalyst to coupling and electric field-synergy, the silicon carbide substrate is supported by loading active ingredients such as palladium oxide, cobalt oxide and platinum oxide on the silicon carbide substrate, and applying milliamper current using the electric field to achieve efficient catalytic oxidation of volatile organic compounds. , reduce the amount of precious metals.
Under the condition of no more than 350V, the low temperature (≤200℃) and high-efficiency oxidation conversion rate (≥90%) of typical volatile organic compounds is achieved, reducing the amount of precious metals by 50%, saving the cost of catalyst research and development, and providing new VOCs emissions Control technology approach.
Smart Images

Figure CN119015848A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalytic oxidation, and in particular relates to a catalytic oxidation method for removing volatile organic matter by utilizing an electric field. Background Art
[0002] There is a low concentration of unburned methane in the exhaust gas of natural gas engines; in the fume of restaurant oils, alkanes, alkenes, aromatic non-methane hydrocarbons and oxygen-containing organic compounds account for about 60% and 30% of the total emissions respectively. These VOCs gases are difficult to collect and utilize, but they are seriously destructive to the environment and harmful to human health. The molecular configuration of methane is a tetrahedral structure. It is the most stable and most difficult to remove hydrocarbon. Its ability to produce a greenhouse effect is 28 times that of carbon dioxide; organic substances such as propane, propylene, benzene, toluene, formaldehyde, and acetaldehyde can seriously endanger human health, among which benzene and formaldehyde are Class 1 carcinogens; acetaldehyde is a Class 2B carcinogen; toluene and propylene are Class 3 carcinogens. Therefore, how to efficiently remove the above VOCs gases under low temperature conditions is one of the problems that urgently need to be solved in the field of vehicle and ship power exhaust, industrial fixed source flue gas, and restaurant fume pollutant control.
[0003] Catalytic oxidation based on precious metal materials is a traditional technical method for removing low-concentration VOCs such as alkanes (methane, propane), olefins (propylene), aromatic hydrocarbons (benzene, toluene, ethylbenzene), oxygen-containing organic matter (formaldehyde, acetaldehyde), etc. However, it is limited by the high cost of catalyst research and development, low efficiency at low temperatures, and easy sintering of precious metals. It is currently difficult to achieve large-scale application in the fields of vehicle and ship power exhaust, industrial fixed-source flue gas, and catering industry oil fume treatment. Summary of the invention
[0004] The object of the present invention is to provide a catalytic oxidation method for removing volatile organic compounds by using an electric field. The catalytic oxidation method provided by the present invention has a high low-temperature catalytic efficiency for volatile organic compounds.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The present invention provides a catalytic oxidation method for removing volatile organic compounds by using an electric field, comprising the following steps:
[0007] Under the action of the electric field, the gas to be treated is catalytically oxidized through the catalyst;
[0008] The gas to be treated includes volatile organic matter, oxygen and nitrogen;
[0009] The catalyst comprises a silicon carbide substrate and a catalyst coating supported on the silicon carbide substrate;
[0010] The material of the catalyst coating includes a carrier and an active component supported on the carrier;
[0011] The active ingredient includes one or more of palladium oxide, cobalt oxide and platinum oxide;
[0012] The support includes ceria, zirconia and alumina.
[0013] Preferably, the mass percentage of the active ingredient in the catalyst coating does not exceed 3wt%;
[0014] The content of the catalyst coating in the silicon carbide-based catalyst is 100 g / L.
[0015] Preferably, the silicon carbide substrate is in a honeycomb shape, the particle size of the silicon carbide substrate is not less than 300 meshes, and the wall thickness is 0.25 mm.
[0016] Preferably, the method for preparing the silicon carbide-based catalyst comprises the following steps:
[0017] The carrier, a noble metal salt solution, a binder, a thickener and water are mixed to obtain a slurry; the noble metal salt solution includes one or more of a palladium salt solution, a cobalt salt solution and a platinum salt solution;
[0018] The slurry is coated on a silicon carbide substrate and calcined to obtain the silicon carbide-based catalyst.
[0019] Preferably, the binder comprises methyl cellulose, and the mass of the binder does not exceed 0.6% of the mass of the slurry;
[0020] The thickener comprises pseudo-boehmite, and the mass of the thickener does not exceed 6% of the mass of the slurry.
[0021] Preferably, the calcination temperature is 400° C. to 600° C., and the holding time is 3 to 6 hours.
[0022] Preferably, the volume concentration of volatile organic matter in the gas to be treated is ≤0.1%, and the volume concentration of oxygen is 10.0%.
[0023] Preferably, the space velocity of the gas to be treated is 10000~100000h -1 .
[0024] Preferably, the temperature of the catalyst in the catalytic oxidation is ≤200°C.
[0025] Preferably, the voltage of the electric field is 100-350V, and the current is 25-200mA.
[0026] The present invention provides a catalytic oxidation method for removing volatile organic matter by using an electric field, comprising the following steps: catalytically oxidizing a gas to be treated through a catalyst under the action of an electric field; the gas to be treated comprises volatile organic matter, oxygen and nitrogen; the catalyst comprises a silicon carbide substrate and a catalyst coating supported on the silicon carbide substrate; the material of the catalyst coating comprises a carrier and an active component supported on the carrier; the active component comprises one or more of palladium oxide, cobalt oxide and platinum oxide; the carrier comprises cerium oxide, zirconium oxide and aluminum oxide. The present invention utilizes the coupling-synergistic effect of silicon carbide-based catalysts and electric fields to effectively reduce the amount of precious metals used, applies milliampere current to the catalyst surface, and achieves efficient oxidation (conversion rate ≥ 90%) of typical alkanes, olefins, aromatic hydrocarbons and oxygen-containing organic matter at low temperatures (≤ 200°C) under voltage conditions not exceeding 350V; and compared with thermal catalytic systems, it can reduce the amount of precious metals used by at least 50%, saving catalyst research and development costs, and providing a new technical approach for various fields or scenarios that require control of volatile organic compounds (VOCs) emissions. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The schematic diagram of the structure of the device used for catalytic oxidation in the present invention, wherein 1 is a volatile organic dilution gas cylinder, 2 is a high-purity oxygen cylinder, 3 is a high-purity nitrogen cylinder, 4 is a mass flow controller, 5 is a stainless steel electrode, 6 is a stainless steel ferrule, 7 is a thermocouple, 8 is a catalyst, 9 is a grounding wire, 10 is a high-voltage DC power supply, and 11 is a Fourier transform infrared spectrometer. DETAILED DESCRIPTION
[0028] The present invention provides a catalytic oxidation method for removing volatile organic compounds by using an electric field, comprising the following steps:
[0029] Under the action of the electric field, the gas to be treated is catalytically oxidized through the catalyst;
[0030] The gas to be treated includes volatile organic matter, oxygen and nitrogen;
[0031] The catalyst comprises a silicon carbide substrate and a catalyst coating supported on the silicon carbide substrate;
[0032] The material of the catalyst coating includes a carrier and an active component supported on the carrier;
[0033] The active ingredient includes one or more of palladium oxide, cobalt oxide and platinum oxide;
[0034] The support includes ceria, zirconia and alumina.
[0035] In the present invention, the silicon carbide substrate is preferably in a honeycomb shape, the particle size of the silicon carbide substrate is preferably not less than 300 meshes, and the wall thickness is preferably 0.25 mm. In the present invention, the silicon carbide substrate is preferably prepared by a recrystallization method or a chemical sintering method. The present invention has no special restrictions on the specific processes of the recrystallization method and the chemical sintering method, and those familiar to those skilled in the art can be used.
[0036] In the present invention, the aluminum oxide is preferably γ-alumina. In the present invention, the mass ratio of cerium oxide to zirconium oxide in the carrier is preferably 0.25 to 3:1; the mass ratio of the total mass of cerium oxide and zirconium oxide in the carrier to aluminum oxide is preferably 0.5 to 4:1. In the present invention, the mass percentage of the active ingredient in the catalyst coating is preferably no more than 3wt%.
[0037] In the present invention, the content of the catalyst coating in the silicon carbide-based catalyst is preferably 100 g / L.
[0038] The present invention uses silicon carbide as a substrate and utilizes its conductive properties in an electric field to greatly improve the catalytic oxidation efficiency of typical alkanes, olefins, aromatic hydrocarbons, and oxygen-containing organic matter including methane.
[0039] In the present invention, the method for preparing the silicon carbide-based catalyst preferably comprises the following steps:
[0040] The carrier, a noble metal salt solution, a binder, a thickener and water are mixed to obtain a slurry; the noble metal salt solution includes one or more of a palladium salt solution, a cobalt salt solution and a platinum salt solution;
[0041] The slurry is coated on a silicon carbide substrate and calcined to obtain the silicon carbide-based catalyst.
[0042] The invention mixes a carrier, a noble metal salt solution, a binder, a thickener and water to obtain a slurry; the noble metal salt solution comprises one or more of a palladium salt solution, a cobalt salt solution and a platinum salt solution.
[0043] In the present invention, the binder preferably includes methyl cellulose, and the mass of the binder preferably does not exceed 0.6% of the mass of the slurry; the thickener preferably includes pseudo-boehmite, and the mass of the thickener preferably does not exceed 6% of the mass of the slurry.
[0044] In the present invention, the palladium salt solution is preferably a palladium nitrate solution; the cobalt salt solution is preferably a cobalt nitrate solution; and the platinum salt solution is preferably a platinum nitrate solution. The present invention has no particular limitation on the concentration of the noble metal salt solution, and any concentration known to those skilled in the art may be used. The present invention has no particular limitation on the solid content of the slurry, and any concentration known to those skilled in the art may be used.
[0045] In the present invention, the mixing order is preferably: after the carrier and water are stirred at a constant temperature, the noble metal salt solution, the binder and the thickener are added and stirred and mixed. In the present invention, the temperature of the constant temperature stirring is preferably 30°C, the time is preferably 1 hour; the stirring and mixing time is preferably 1 hour.
[0046] After obtaining the slurry, the present invention coats the slurry on a silicon carbide substrate and obtains the silicon carbide-based catalyst after calcination.
[0047] The present invention has no special limitation on the coating process, and a method known to those skilled in the art can be used. In the present invention, the calcination temperature is preferably 400-600°C, more preferably 550°C; the holding time is preferably 3-6h, more preferably 4h. In the present invention, the calcination is preferably carried out in a muffle furnace.
[0048] In the present invention, the volatile organic matter preferably includes one or more of alkanes, olefins, aromatic hydrocarbons and oxygen-containing organic matter; the alkanes preferably include methane and / or propane, the olefins preferably include propylene, the aromatic hydrocarbons preferably include one or more of benzene, toluene and ethylbenzene, and the oxygen-containing organic matter preferably includes formaldehyde and / or acetaldehyde.
[0049] In the present invention, the volume concentration of volatile organic matter in the gas to be treated is preferably ≤0.1%, the volume concentration of oxygen is preferably 10.0%; the remainder is preferably nitrogen. In the present invention, the space velocity of the gas to be treated is preferably 10000~100000h -1 , preferably 10000h -1 、30000h -1 、50000h -1 or 100000h -1 .
[0050] In the present invention, the temperature of the catalyst in the catalytic oxidation is preferably ≤ 200° C. In the present invention, the voltage of the electric field is preferably 100 to 350 V, and the current is preferably 25 to 200 mA. In the present invention, the current mode during the catalytic oxidation is preferably a constant current mode.
[0051] In the present invention, the reaction in the catalytic oxidation process preferably includes:
[0052] CH4+2O2=CO2+2H2O;
[0053] C3H8+5O2=3CO2+4H2O;
[0054] 2C3H6+9O2=6CO2+6H2O;
[0055] 2C6H6+15O2=12CO2+6H2O;
[0056] C7H8+9O2=7CO2+4H2O;
[0057] CH2O+O2=CO2+H2O;
[0058] 2C2H4O+5O2=4CO2+4H2O.
[0059] In the present invention, the structural schematic diagram of the device used for catalytic oxidation is as follows Figure 1 As shown, 1 is a volatile organic dilution gas cylinder, 2 is a high-purity oxygen cylinder, 3 is a high-purity nitrogen cylinder, 4 is a mass flow controller, 5 is a stainless steel electrode, 6 is a stainless steel ferrule, 7 is a thermocouple, 8 is a catalyst, 9 is a grounding wire, 10 is a high-voltage DC power supply, and 11 is a Fourier transform infrared spectrometer.
[0060] In the present invention, the size of the catalyst in the device is preferably: length*width*height≥7*5*20mm.
[0061] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.
[0062] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0063] Example 1
[0064] Disperse cerium dioxide (CeO2), zirconium dioxide (ZrO2) and γ-alumina (γ-Al2O3) in a mass ratio of 1:1:1 in deionized water, and stir at 30°C for 1 hour; add palladium nitrate solution, methyl cellulose and pseudo-boehmite, and stir and mix for 1 hour to obtain a slurry, wherein the mass of methyl cellulose is 0.3% of the mass of the slurry, and the mass of pseudo-boehmite is 3% of the mass of the slurry;
[0065] The slurry was coated on a silicon carbide substrate (the particle size of the silicon carbide substrate was 300 mesh and the wall thickness was 0.25 mm), and then transferred into a muffle furnace and calcined at 550° C. for 4 h to obtain the silicon carbide-based catalyst, wherein the content of the catalyst coating in the silicon carbide-based catalyst was 100 g / L, the content of palladium oxide in the catalyst coating was 1 wt%, and the obtained silicon carbide-based catalyst was recorded as 1 wt% PdO x / CeO2-ZrO2-γ-Al2O3 / SiC.
[0066] use Figure 1 The obtained catalyst is used to catalytically oxidize methane, propane and propylene respectively; wherein the volume concentration of oxygen in the gas to be treated is 10%, the volume concentration of methane, propane and propylene is set to 0.10%, and the space velocity is 50000h -1 ; The size of the catalyst in the device is 7*5*20mm;
[0067] The methane conversion rate (expressed as X1%), propane conversion rate (expressed as X2%) and propylene conversion rate (expressed as X3%) under different current conditions (25mA, 50mA, 75mA, 100mA, 150mA, 200mA) are used as evaluation criteria for the performance of the silicon carbide-based catalyst in the electric field; the electric current will produce a thermal effect, resulting in different catalyst bed temperatures under different current conditions. In order to compare with the thermal catalytic conversion process, the bed temperature under 25mA, 50mA, 75mA, 100mA, 150mA, and 200mA conditions is used as the reaction temperature in the thermal catalytic system to test the methane conversion rate (expressed as N1%), propane conversion rate (expressed as N2%), and propylene (expressed as N3%) as evaluation criteria for the catalyst reaction performance under thermal catalytic conditions;
[0068] The test conditions and the obtained test results are shown in Table 1;
[0069] Table 1 Conversion rates of methane, propane and propylene over silicon carbide-based catalysts
[0070]
[0071] Based on the CeO2-ZrO2-γ-Al2O3 blank carrier, that is, no active ingredients are loaded, when the electric field is applied alone, the conversion rates of methane, propane and propylene are all zero under different current conditions.
[0072] Example 2
[0073] A silicon carbide-based catalyst was prepared in the manner of Example 1, wherein the active ingredient was 2 wt% PdO x The obtained silicon carbide-based catalyst is recorded as 2wt% PdO x / CeO2-ZrO2-γ-Al2O3 / SiC.
[0074] Methane, propane and propylene were catalytically oxidized in the manner of Example 1. The test conditions and test results are shown in Table 2.
[0075] Table 2 Conversion of methane, propane and propylene over silicon carbide-based catalysts
[0076]
[0077] Based on the CeO2-ZrO2-γ-Al2O3 blank carrier, that is, no active ingredients are loaded, when the electric field is applied alone, the conversion rates of methane, propane and propylene are all zero under different current conditions.
[0078] Example 3
[0079] A silicon carbide-based catalyst was prepared in the manner of Example 1, wherein the active ingredient was 1 wt% PdO x and 5wt%CoO x The obtained silicon carbide-based catalyst is denoted as 1wt% PdO x -5wt%CoO x / CeO2-ZrO2-γ-Al2O3 / SiC.
[0080] Methane, propane and propylene were catalytically oxidized in the manner of Example 1. The test conditions and test results are shown in Table 3.
[0081] Table 3 Conversion of methane, propane and propylene over silicon carbide-based catalysts
[0082]
[0083] The test results of the conversion rates of methane, propane and propylene by the catalyst obtained in this example at a current of 100 mA and different space velocities are shown in Table 4;
[0084] Table 4 Conversion of methane, propane and propylene over silicon carbide-based catalysts at different space velocities
[0085]
[0086] Example 4
[0087] A silicon carbide-based catalyst was prepared in the manner of Example 1, wherein the active component was 0.5 wt% PtO x The obtained silicon carbide-based catalyst is recorded as 0.5wt% PtO x / CeO2-ZrO2-γ-Al2O3 / SiC;
[0088] use Figure 1 The obtained catalyst is used to catalytically oxidize benzene, toluene and ethylbenzene respectively; wherein the volume concentration of oxygen in the gas to be treated is 10%, the volume concentration of benzene, toluene and ethylbenzene is set to 0.10%, and the space velocity is 50000h -1 ; The size of the catalyst in the device is 7*5*20mm;
[0089] The benzene conversion rate (expressed as X1%), toluene conversion rate (expressed as X2%) and ethylbenzene conversion rate (expressed as X3%) under different current conditions (25mA, 50mA, 75mA, 100mA, 150mA, 200mA) are used as evaluation criteria for the performance of the silicon carbide-based catalyst in the electric field; the electric current will produce a thermal effect, resulting in different catalyst bed temperatures under different current conditions. In order to compare with the thermal catalytic conversion process, the bed temperature under 25mA, 50mA, 75mA, 100mA, 150mA, and 200mA conditions is used as the reaction temperature in the thermal catalytic system to test the benzene conversion rate (expressed as N1%), toluene conversion rate (expressed as N2%), and ethylbenzene (expressed as N3%) as evaluation criteria for the reaction performance of the catalyst under thermal catalytic conditions;
[0090] The test conditions and the obtained test results are shown in Table 5;
[0091] Table 5 Conversion of benzene, toluene and ethylbenzene over silicon carbide-based catalysts
[0092]
[0093] Example 5
[0094] A silicon carbide-based catalyst was prepared in the manner of Example 4, wherein the active component was 1.0 wt% PtO x The obtained silicon carbide-based catalyst is recorded as 1.0 wt% PtO x / CeO2-ZrO2-γ-Al2O3 / SiC;
[0095] Benzene, toluene and ethylbenzene were catalytically oxidized in the manner of Example 4. The test conditions and test results are shown in Table 6.
[0096] Table 6 Conversion of benzene, toluene and ethylbenzene over silicon carbide-based catalysts
[0097]
[0098] The test results of the conversion of benzene, toluene and ethylbenzene by the catalyst obtained in this example at a current of 100 mA and different space velocities are shown in Table 7;
[0099] Table 7 Conversion of benzene, toluene and ethylbenzene over silicon carbide-based catalysts at different space velocities
[0100]
[0101] Example 6
[0102] A silicon carbide-based catalyst was prepared in the manner of Example 4, wherein the active component was 2.0 wt% PtO xThe obtained silicon carbide-based catalyst is recorded as 2.0 wt% PtO x / CeO2-ZrO2-γ-Al2O3 / SiC;
[0103] Benzene, toluene and ethylbenzene were catalytically oxidized in the manner of Example 4. The test conditions and test results are shown in Table 8.
[0104] Table 8 Conversion rate of catalyst to benzene, toluene and ethylbenzene
[0105]
[0106] Example 7
[0107] A silicon carbide-based catalyst was prepared in the manner of Example 1, wherein the active ingredient was 0.5 wt% PtO x and 1.5wt% PdO x The obtained silicon carbide-based catalyst is recorded as 0.5wt% PtO x -1.5wt% PdO x / CeO2-ZrO2-γ-Al2O3 / SiC;
[0108] use Figure 1 The obtained catalyst is used to catalytically oxidize formaldehyde and acetaldehyde respectively; wherein the volume concentration of oxygen in the gas to be treated is 10%, the volume concentration of formaldehyde and acetaldehyde is set to 0.10%, and the space velocity is 50000h -1 ; The size of the catalyst in the device is 7*5*20mm;
[0109] The formaldehyde conversion rate (expressed as X1%) and acetaldehyde conversion rate (expressed as X2%) under different current conditions (25mA, 50mA, 75mA, 100mA, 150mA, 200mA) were used as evaluation criteria for the performance of the silicon carbide-based catalyst in the electric field; the electric current will produce a thermal effect, resulting in different catalyst bed temperatures under different current conditions. In order to compare with the thermal catalytic conversion process, the bed temperature under 25mA, 50mA, 75mA, 100mA, 150mA, and 200mA conditions was used as the reaction temperature in the thermal catalytic system to test the formaldehyde conversion rate (expressed as N1%) and acetaldehyde conversion rate (expressed as N2%) as evaluation criteria for the catalyst reaction performance under thermal catalytic conditions;
[0110] The test conditions and the obtained test results are shown in Table 9;
[0111] Table 9 Conversion rate of formaldehyde and acetaldehyde by silicon carbide based catalyst
[0112]
[0113] Example 8
[0114] A silicon carbide-based catalyst was prepared in the manner of Example 7, wherein the active ingredient was 1.0 wt% PtO x and 1.0wt% PdO x The obtained silicon carbide-based catalyst is recorded as 1.0 wt% PtO x -1.0wt% PdO x / CeO2-ZrO2-γ-Al2O3 / SiC;
[0115] Formaldehyde and acetaldehyde were catalytically oxidized in the manner of Example 7. The test conditions and test results are shown in Table 10.
[0116] Table 10 Conversion rate of silicon carbide-based catalyst to formaldehyde and acetaldehyde
[0117]
[0118]
[0119] Example 9
[0120] A silicon carbide-based catalyst was prepared in the manner of Example 7, wherein the active ingredient was 1.5 wt% PtO x and 0.5wt% PdO x The obtained silicon carbide-based catalyst is recorded as 1.5wt% PtO x -0.5wt%PdO x / CeO2-ZrO2-γ-Al2O3 / SiC;
[0121] Formaldehyde and acetaldehyde were catalytically oxidized in the manner of Example 7. The test conditions and test results are shown in Table 11.
[0122] Table 11 Conversion rate of formaldehyde and acetaldehyde by silicon carbide based catalyst
[0123]
[0124] The test results of the conversion rates of formaldehyde and acetaldehyde by the catalyst obtained in this example at a current of 100 mA and different space velocities are shown in Table 12;
[0125] Table 12 Conversion rate of formaldehyde and acetaldehyde by silicon carbide-based catalyst at different space velocities
[0126]
[0127] In summary, it can be seen that compared with the prior art, the catalyst provided by the present invention can significantly improve the catalytic oxidation efficiency of representative volatile VOCs such as low-concentration methane, non-methane hydrocarbons (propane, propylene, benzene, toluene, ethylbenzene) and oxygen-containing organic matter (formaldehyde, acetaldehyde) at low temperatures (≤200°C).
[0128] According to Examples 1 to 3, it can be seen that the airspeed condition is set to 50000h -1 , 1wt% PdO on SiC substrate x -5wt%CoO x Under the coupling-synergistic effect of the / CeO2-ZrO2-γ-Al2O3 / SiC catalyst and the electric field (current condition set to 100mA), the catalytic efficiency of alkanes and alkenes such as methane, propane, and propylene is greatly improved compared to the thermal catalytic efficiency at the same temperature. At a catalyst temperature of 200°C, the methane conversion rate is 93.77% (the thermal catalytic methane conversion rate at the same bed temperature is 0%), the propane conversion rate is 94.02% (the thermal catalytic methane conversion rate at the same bed temperature is 5.34%), and the propylene conversion rate is 98.00% (the thermal catalytic methane conversion rate at the same bed temperature is 76.11%); at 100,000h -1 At a high space velocity of 170°C catalyst temperature, the methane conversion rate is 80.31% (the thermal catalytic methane conversion rate at the same bed temperature is 0%), the propane conversion rate is 82.21% (the thermal catalytic methane conversion rate at the same bed temperature is 0.30%), and the propylene conversion rate is 85.41% (the thermal catalytic methane conversion rate at the same bed temperature is 34.11%).
[0129] Set the airspeed condition to 50000h -1 , 2wt% PdO on SiC substrate x Under the coupling and synergistic effect of / CeO2-ZrO2-γ-Al2O3 / SiC catalyst and electric field (current condition set to 100mA), the methane conversion rate at 199°C bed temperature is 93.86% (the thermal catalytic methane conversion rate at the same bed temperature is zero), the propane conversion rate is 95.11% (the thermal catalytic methane conversion rate at the same bed temperature is 7.20%), and the propylene conversion rate is 98.30% (the thermal catalytic methane conversion rate at the same bed temperature is 85.23%).
[0130] In an electric field, 1wt% PdO x -5wt%CoO x / CeO2-ZrO2-γ-Al2O3 / SiC with 2wt% PdO x The removal efficiencies of methane, propane, and propylene over the CeO2-ZrO2-γ-Al2O3 / SiC catalysts are almost the same, which proves that the removal efficiency of methane, propane, and propylene over the 5wt% CoO2 / SiC catalysts is almost the same. xDoping can reduce the amount of precious metals used by 50%, saving the R&D cost of the catalyst.
[0131] According to Examples 4 to 6, it can be seen that the airspeed condition is set to 50000h -1 , 1wt% PtO on SiC substrate x Under the coupling-synergistic effect of / CeO2-ZrO2-γ-Al2O3 / SiC catalyst and electric field (current condition set at 25mA), the catalytic efficiency of aromatic hydrocarbons such as benzene, toluene, and ethylbenzene is greatly improved compared with the thermal catalytic efficiency at the same temperature. At a bed temperature of 130°C, the benzene conversion rate is 89.32% (the thermal catalytic methane conversion rate at the same bed temperature is 13.32%), the toluene conversion rate is 90.11% (the thermal catalytic methane conversion rate at the same bed temperature is 20.34%), and the ethylbenzene conversion rate is 92.31% (the thermal catalytic methane conversion rate at the same bed temperature is 28.08%).
[0132] According to Examples 7 to 9, it can be seen that the airspeed condition is set to 50000h -1 , 1wt% PtO on SiC substrate x -1wt% PdO x Under the coupling and synergistic effect of the / CeO2-ZrO2-γ-Al2O3 / SiC catalyst and the electric field (current condition set at 25mA), the catalytic efficiency of oxygen-containing organic matter such as formaldehyde and acetaldehyde is greatly improved compared with the thermal catalytic efficiency at the same temperature. At a bed temperature of 129°C, the formaldehyde conversion rate is 79.31% (the thermal catalytic methane conversion rate at the same bed temperature is 28.73%), and the acetaldehyde conversion rate is 90.21% (the thermal catalytic methane conversion rate at the same bed temperature is 38.75%); under the current condition of 100mA and the bed temperature of 173°C, both can be completely converted.
[0133] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A catalytic oxidation method for removing volatile organic compounds using an electric field, characterized in that: The following steps are involved: Under the action of the electric field, the gas to be treated is catalytically oxidized through the catalyst; The gas to be treated includes volatile organic matter, oxygen and nitrogen; The catalyst comprises a silicon carbide substrate and a catalyst coating supported on the silicon carbide substrate; The material of the catalyst coating includes a carrier and an active component supported on the carrier; The active ingredient includes one or more of palladium oxide, cobalt oxide and platinum oxide; The support includes ceria, zirconia and alumina.
2. The catalytic oxidation method according to claim 1, characterized in that: The mass percentage of the active ingredient in the catalyst coating does not exceed 3wt%; The content of the catalyst coating in the silicon carbide-based catalyst is 100 g / L.
3. The catalytic oxidation method according to claim 1, characterized in that: The silicon carbide substrate is in a honeycomb shape, the particle size of the silicon carbide substrate is not less than 300 meshes, and the wall thickness is 0.25 mm.
4. The catalytic oxidation method according to claim 1, characterized in that: The method for preparing the silicon carbide-based catalyst comprises the following steps: The carrier, a noble metal salt solution, a binder, a thickener and water are mixed to obtain a slurry; the noble metal salt solution includes one or more of a palladium salt solution, a cobalt salt solution and a platinum salt solution; The slurry is coated on a silicon carbide substrate and calcined to obtain the silicon carbide-based catalyst.
5. The catalytic oxidation method according to claim 4, characterized in that: The binder includes methyl cellulose, and the mass of the binder does not exceed 0.6% of the mass of the slurry; The thickener comprises pseudo-boehmite, and the mass of the thickener does not exceed 6% of the mass of the slurry.
6. The catalytic oxidation method according to claim 4, characterized in that: The calcination temperature is 400° C. to 600° C., and the heat preservation time is 3 to 6 hours.
7. The catalytic oxidation method according to claim 1, characterized in that: The volume concentration of volatile organic matter in the gas to be treated is ≤0.1%, and the volume concentration of oxygen is 10.0%.
8. The catalytic oxidation method according to claim 1 or 7, characterized in that: The space velocity of the gas to be treated is 10000~100000h -1 .
9. The catalytic oxidation method according to claim 1, characterized in that: The temperature of the catalyst in the catalytic oxidation is ≤200°C.
10. The catalytic oxidation method according to claim 1, characterized in that: The voltage of the electric field is 100-350V, and the current is 25-200mA.