Selective mineralization-gradient recovery method for valuable components in manganese residue leachate

By using manganese carbonate particles and sodium dihydrogen phosphate precipitation technology in manganese slag leachate, manganese, magnesium ions and ammonia nitrogen is selectively separated and recovered, and the problem of difficult recovery of valuable components in manganese slag leachate is solved, achieving high efficiency staircase recycling and pollution reduction.

CN119020592APending Publication Date: 2024-11-26CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410913468.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-22
Filing Date
2024-07-09
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to selectively separate and recover valuable components such as manganese, magnesium ions and ammonia nitrogen in manganese slag leachate, resulting in water and soil pollution, and it is difficult to achieve step-by-step recovery of manganese slag leachate.

Method used

Manganese carbonate particles are used as crystal nucleus to precipitate manganese ions through carbonate, and magnesium ions and ammonia nitrogen are precipitated with sodium dihydrogen phosphate to form stable struvite precipitation, and then calcination and separation of magnesium and ammonia nitrogen are achieved to achieve selective mineralization-stage recovery .

Benefits of technology

It significantly improves the separation efficiency and recovery efficiency of valuable components, reduces raw material consumption, and promotes the formation and growth of manganese carbonate crystals, shortens the reaction time, and improves the yield and quality of the crystals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020592A_ABST
    Figure CN119020592A_ABST
Patent Text Reader

Abstract

The invention relates to a selective mineralization-gradient recovery method for valuable components in manganese residue leachate. Belongs to the technical field of heavy metal harmless and resourceful treatment. According to the method, firstly, manganese carbonate particles serve as crystal nucleuses, carbonate is adopted for selective precipitation of manganese ions, then sodium dihydrogen phosphate is added for precipitation of magnesium ions and ammonia nitrogen, stable struvite precipitation is formed, finally, the precipitation is roasted to separate magnesium and ammonia nitrogen, and finally selective mineralization-gradient recovery of valuable components in the manganese residue leachate is achieved. The separation efficiency and the valuable component recovery efficiency are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a selective mineralization-cascade recovery method for valuable components in manganese slag leachate, and belongs to the technical field of harmless and resourceful treatment of heavy metals. Background Art

[0002] Manganese is one of my country's important strategic resources. Most of the manganese in my country is consumed in the steel industry to improve the strength of steel. Metallic manganese is usually extracted by thermal or electrolytic methods. The purity of metal manganese prepared by electrolytic manganese is higher, but a large amount of electrolytic manganese slag will be produced in the process of electrolytic manganese. In addition, early electrolytic manganese enterprises piled up electrolytic manganese slag in the open air for a long time. In this process, a large amount of electrolytic manganese slag leachate was produced due to rainwater leaching. The manganese slag leachate contains a large amount of manganese, magnesium ions and ammonia nitrogen. Due to the lack of anti-seepage measures, it is very easy to cause the spread of electrolytic manganese slag leachate, causing water and soil pollution. Excessive intake of manganese by the human body will cause damage to the extrapyramidal tract of the nervous system and Parkinson's disease syndrome. Acute manganese poisoning manifests itself as headache, chest tightness, chills, dystonia and other symptoms. In addition, ammonia nitrogen is easily decomposed into nitrite nitrogen by microorganisms in water bodies. Nitrite nitrogen combines with proteins in the human body to form nitrosamines. If the human body drinks water with excessive ammonia nitrogen for a long time, it will cause poisoning to the human body, and it also has carcinogenic effects. It is urgent to render it harmless and recycle it into resources.

[0003] At present, there are two common methods for treating ammonia nitrogen in manganese slag leachate: physical and chemical method and biological method. The physical and chemical method mainly includes: stripping gas stripping method, chemical precipitation method, breakpoint chlorination method, struvite precipitation method, etc. The biological method mainly includes simultaneous nitrification and denitrification method, traditional biological denitrification method, etc. The treatment method of manganese ions in the solution mainly adopts precipitation method, which mainly includes: sulfide precipitation method, carbonate precipitation method, hydroxide precipitation method, oxidation precipitation method, etc. The struvite precipitation method has the advantage of removing magnesium ions and ammonia nitrogen at the same time, but in the process of removing high-concentration manganese ions, dense manganese phosphate precipitates will be generated, which is difficult to separate solid and liquid, thereby affecting the subsequent removal of magnesium ions and ammonia nitrogen, making it difficult to achieve the cascade recovery of valuable components in manganese slag leachate. Summary of the invention

[0004] In view of the difficulty that valuable components (manganese, magnesium ions and ammonia nitrogen, etc.) in manganese-containing wastewater cannot be selectively separated and recovered, the present invention provides a technical prototype for selective mineralization-step recovery of valuable components in manganese slag leachate. First, manganese carbonate particles are used as crystal nuclei to selectively precipitate manganese ions with carbonates, and then sodium dihydrogen phosphate is added to precipitate magnesium ions and ammonia nitrogen to form a stable struvite precipitate. Finally, the precipitate is roasted to separate magnesium and ammonia nitrogen, and finally selective mineralization-step recovery of valuable components in manganese slag leachate is achieved, and the separation efficiency and the recovery efficiency of valuable components are greatly increased.

[0005] In order to achieve the above object, the present invention provides a method for selective mineralization and cascade recovery of valuable components in manganese slag leachate, which comprises the following steps:

[0006] Add 0.02-3.5g of sodium carbonate and 0.01-2.5g of 400-800 mesh manganese carbonate to 100ml of manganese slag leachate; add sodium carbonate and manganese carbonate to the manganese slag leachate, and use a pH adjuster (sodium hydroxide, etc.) to adjust the pH to 7-7.5, and stir magnetically for 4-5h at 40-50°C to produce manganese carbonate precipitation, filter, and recover the precipitated slag and the filtrate after solid-liquid separation.

[0007] Mn 2+ +CO3 2- =MnCO3;

[0008] Magnesium ions and ammonia nitrogen components are also present in the filtrate. Sodium dihydrogen phosphate is added in a ratio of 0.2-12 g of sodium dihydrogen phosphate per 100 ml, the pH is adjusted to between 9.5 and 10, and magnetic stirring is performed for 15-30 minutes to produce a stable struvite precipitate.

[0009] Mg 2+ +NH4 + +HPO4 2- +6H2O→MgNH4PO4·6H2O↓+H + .

[0010] The main component of the precipitated slag obtained in step (1) is manganese carbonate, which can be used for the next step of smelting, or the precipitated slag can be ground to 400-800 mesh and directly used as a crystal nucleus to induce the formation of the precipitate in step one.

[0011] Preferably, in the present invention, when the manganese ion concentration in the manganese slag leachate is less than or equal to 0.5 g / l, sodium carbonate and manganese carbonate are added in a ratio of 0.02-0.5 g sodium carbonate to 0.01-0.05 g 400-800 mesh manganese carbonate to 100 ml manganese slag leachate.

[0012] Preferably, in the present invention, when the manganese ion concentration in the manganese slag leachate is 10-15 g / l, sodium carbonate and manganese carbonate are added in a ratio of 2-3.5 g sodium carbonate to 1-2.5 g 400-800 mesh manganese carbonate in 100 ml manganese slag leachate.

[0013] Preferably, in the present invention, when the magnesium ion content in the manganese slag leachate is less than or equal to 0.5 g / l and the ammonia nitrogen content is less than or equal to 0.5 g / l, in step (2), sodium dihydrogen phosphate is added at a ratio of 0.2-1 g of sodium dihydrogen phosphate to 100 ml of liquid.

[0014] Preferably, in the present invention, when the magnesium ion content in the manganese slag leachate is greater than or equal to 5 g / l and the ammonia nitrogen content is less than or equal to 5 g / l, in step (2), sodium dihydrogen phosphate is added at a ratio of 7-12 g of sodium dihydrogen phosphate to 100 ml of liquid.

[0015] The struvite precipitate obtained in step (2) is roasted to obtain roasted slag, the main component of which is magnesium phosphate.

[0016] Principles and advantages

[0017] In the present invention, carbonate can selectively adsorb with manganese ions under appropriate conditions and can form a stable manganese carbonate precipitation in a sufficiently long time, so as to separate manganese ions from magnesium ions and ammonia nitrogen. Manganese carbonate can be recycled as a raw material of the electrolytic manganese process, and the precipitated slag is ground to 400-800 mesh, which can be directly used as a crystal nucleus to induce the formation of manganese carbonate precipitation. The presence of the precipitated crystal nucleus helps to promote the formation and growth of manganese carbonate crystals, improve the yield and quality of the crystals, and shorten the reaction time. Under the condition of the presence of phosphate, ammonia nitrogen and magnesium ions and phosphates undergo precise mineralization precipitation. In the process of roasting struvite, the ammonia generated during roasting is recovered and can also be directly used in the process of electrolytic manganese, reducing the consumption of raw materials.

[0018] The invention has a remarkable effect when treating manganese slag leachate with low manganese ion concentration, low magnesium ion concentration and low ammonia nitrogen content, and the dosage of manganese carbonate crystal nucleus, sodium carbonate and sodium dihydrogen phosphate is also very small. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Flow chart of the process designed for the present invention. DETAILED DESCRIPTION

[0020] Example 1

[0021] The initial manganese slag leachate has a pH of 4.5, a manganese ion content of 13.89 g / l, a magnesium ion content of 14.13 g / l, and an ammonia nitrogen content of 6.27 g / l. 100 ml of manganese slag leachate is added to a beaker, and 1 g of manganese carbonate with a particle size of 400-800 mesh is added as a crystal nucleus; 2.95 g of sodium carbonate is added, and the pH is adjusted to 7.3. In a sealed environment at 40 ° C, the magnetic reaction is carried out for 4 hours, and the manganese ion content drops to 0.99 g / l, and the manganese recovery rate is 9 The content of magnesium ion is 2.8%, and the content of magnesium ion is 13.58g / l. The filter residue is mainly composed of manganese carbonate and a small amount of magnesium carbonate, which can be returned to the electrolytic cell as a raw material for electrolytic manganese for repeated utilization. 9.98g of sodium dihydrogen phosphate is added to the filtrate, the pH is adjusted to 9.5, and the reaction is carried out for 15min. The filter residue obtained after filtration is mainly magnesium ammonium phosphate. The content of manganese ion after the reaction is 0.483g / l, the content of magnesium ion is 0.367g / l, and the recovery rate of magnesium is 97.2%.

[0022] Example 2

[0023] The initial manganese slag leachate has a pH of 4.71, a manganese ion content of 119.17 mg / l, a magnesium ion content of 374.53 mg / l, and an ammonia nitrogen content of 102.02 mg / l. 100 ml of manganese slag leachate is added to a beaker, and 0.02 g of manganese carbonate with a particle size of 400-800 mesh is added as a crystal nucleus; 0.025 g of sodium carbonate is added, and the pH is adjusted to 7.26. The reaction is carried out under magnetic stirring at 40 ° C in a sealed environment for 4 hours, and the manganese ion content drops to 9.86 mg / l. The magnesium ion content is 358.61 mg / l, the filter residue is mainly composed of manganese carbonate, the manganese recovery rate is 91.72%, and a small amount of magnesium carbonate can be returned to the electrolytic cell as a raw material for electrolytic manganese for repeated utilization. 0.26 g of sodium dihydrogen phosphate is added to the filtrate, the pH is adjusted to 9.62, and the reaction is carried out for 15 minutes. The filter residue obtained after filtration is mainly magnesium ammonium phosphate. After the reaction, the manganese ion content is 2.83 mg / l, the magnesium ion content is 12.57 mg / l, and the magnesium recovery rate is 96.5%.

[0024] Example 3

[0025] The initial manganese slag leachate has a pH of 4.71, a manganese ion content of 10.32 g / l, a magnesium ion content of 11.24 g / l, and an ammonia nitrogen content of 5.4 g / l. 100 ml of manganese slag leachate is added to a beaker, and 1 g of manganese carbonate with a particle size of 400-800 mesh is added as a crystal nucleus; 2.18 g of sodium carbonate is added, and the pH is adjusted to 7.45. In a sealed environment at 40°C, the magnetic reaction is carried out for 4 hours, and the manganese ion content drops to 0.85 g / l, and the manganese recovery rate is The content of magnesium ion is 91.76%, and the content of magnesium ion is 10.96g / l. The filter residue is mainly composed of manganese carbonate and a small amount of magnesium carbonate, which can be returned to the electrolytic cell as a raw material for electrolytic manganese for repeated utilization. 8.03g of sodium dihydrogen phosphate is added to the filtrate, and the pH is adjusted to 9.7. The reaction is carried out for 15 minutes. The filter residue obtained after filtration is mainly magnesium ammonium phosphate. The content of manganese ion after the reaction is 0.32g / l, the content of magnesium ion is 0.28g / l, and the recovery rate of magnesium is 97.4%.

[0026] Example 4

[0027] The initial manganese slag leachate has a pH of 4.5, a manganese ion content of 13.89 g / l, a magnesium ion content of 14.13 g / l, and an ammonia nitrogen content of 6.27 g / l. 100 ml of manganese slag leachate is added to a beaker, and 1 g of manganese carbonate with a particle size of 400-800 mesh is added as a crystal nucleus; 3.1 g of sodium carbonate is added, and the pH is adjusted to 7.6. In a sealed environment at 40 ° C, the magnetic reaction is carried out for 4 hours, and the manganese ion content drops to 1.32 g / l, and the manganese recovery rate is 90 .5%, the magnesium ion content is 13.62g / l, the filter residue is mainly composed of manganese carbonate and a small amount of magnesium carbonate, which can be returned to the electrolytic cell as a raw material for electrolytic manganese for repeated utilization. 9.98g of sodium dihydrogen phosphate is added to the filtrate, the pH is adjusted to 9.5, and the reaction is carried out for 15 minutes. The filter residue obtained after filtration is mainly magnesium ammonium phosphate. After the reaction, the content of manganese ions is 0.492g / l, the content of magnesium ions is 0.875g / l, and the recovery rate of magnesium is 93.6%.

[0028] Example 5

[0029] The initial manganese slag leachate has a pH of 4.5, a manganese ion content of 13.89 g / l, a magnesium ion content of 14.13 g / l, and an ammonia nitrogen content of 6.27 g / l. 100 ml of manganese slag leachate is added to a beaker, and 1 g of manganese carbonate with a particle size of 400-800 mesh is added as a crystal nucleus; 2.6 g of sodium carbonate is added, and the pH is adjusted to 7.5. In a sealed environment at 40°C, the magnetic reaction is carried out for 4.5 hours, and the manganese ion content drops to 1.25 g / l. The manganese recovery rate is 91%, the magnesium ion content is 13.67g / l, the filter residue is mainly composed of manganese carbonate and a small amount of magnesium carbonate, which can be returned to the electrolytic cell as a raw material for electrolytic manganese for repeated utilization. 9.98g of sodium dihydrogen phosphate is added to the filtrate, the pH is adjusted to 9.7, and the reaction is carried out for 15min. The filter residue obtained after filtration is mainly magnesium ammonium phosphate. After the reaction, the content of manganese ions is 0.621g / l, the content of magnesium ions is 0.927g / l, and the recovery rate of magnesium is 93.3%.

[0030] Example 6

[0031] The initial manganese slag leachate has a pH of 4.5, a manganese ion content of 13.89 g / l, a magnesium ion content of 14.13 g / l, and an ammonia nitrogen content of 6.27 g / l. 100 ml of manganese slag leachate is added to a beaker, and 1.3 g of manganese carbonate with a particle size of 400-800 mesh is added as a crystal nucleus; 2.95 g of sodium carbonate is added, and the pH is adjusted to 7.3. In a sealed environment at 40 ° C, the magnetic reaction is carried out for 4 hours, and the manganese ion content drops to 0.93 g / l, and the manganese recovery rate is 9 The content of magnesium ion is 3.3%, and the content of magnesium ion is 13.46g / l. The filter residue is mainly composed of manganese carbonate and a small amount of magnesium carbonate, which can be returned to the electrolytic cell as a raw material for electrolytic manganese for repeated utilization. 10.06g of sodium dihydrogen phosphate is added to the filtrate, and the pH is adjusted to 9.62. The reaction is carried out for 17 minutes. The filter residue obtained after filtration is mainly magnesium ammonium phosphate. The content of manganese ion after the reaction is 0.471g / l, the content of magnesium ion is 0.326g / l, and the recovery rate of magnesium is 97.6%.

[0032] Example 7

[0033] The initial manganese slag leachate has a pH of 4.5, a manganese ion content of 13.89 g / l, a magnesium ion content of 14.13 g / l, and an ammonia nitrogen content of 6.27 g / l. 100 ml of manganese slag leachate is added to a beaker, and 1.6 g of manganese carbonate with a particle size of 400-800 mesh is added as a crystal nucleus; 3.02 g of sodium carbonate is added, and the pH is adjusted to 7.5. In a sealed environment at 40°C, the magnetic reaction is carried out for 4.5 hours, and the manganese ion content drops to 0.89 g / l, and the manganese recovery rate is 93.6%, the magnesium ion content is 13.39g / l, the filter residue is mainly composed of manganese carbonate and a small amount of magnesium carbonate, which can be returned to the electrolytic cell as a raw material for electrolytic manganese for repeated utilization. 10.03g of sodium dihydrogen phosphate is added to the filtrate, the pH is adjusted to 9.76, and the reaction is carried out for 15min. The filter residue obtained after filtration is mainly magnesium ammonium phosphate. After the reaction, the content of manganese ions is 0.481 / l, the content of magnesium ions is 0.359g / l, and the recovery rate of magnesium is 97.3%.

[0034] Example 8

[0035] The initial manganese slag leachate has a pH of 4.5, a manganese ion content of 13.89 g / l, a magnesium ion content of 14.13 g / l, and an ammonia nitrogen content of 6.27 g / l. 100 ml of manganese slag leachate is added to a beaker, and 2 g of manganese carbonate with a particle size of 400-800 mesh is added as a crystal nucleus; 2.85 g of sodium carbonate is added, and the pH is adjusted to 7.1. In a sealed environment at 40 ° C, the magnetic reaction is carried out for 5 hours, and the manganese ion content drops to 0.92 g / l, and the manganese recovery rate is 93 .4%, the magnesium ion content is 13.42g / l, the filter residue is mainly composed of manganese carbonate and a small amount of magnesium carbonate, which can be returned to the electrolytic cell as a raw material for electrolytic manganese for repeated utilization. 9.99g of sodium dihydrogen phosphate is added to the filtrate, the pH is adjusted to 9.83, and the reaction is carried out for 15 minutes. The filter residue obtained after filtration is mainly magnesium ammonium phosphate. After the reaction, the content of manganese ions is 0.479g / l, the content of magnesium ions is 0.364g / l, and the recovery rate of magnesium is 97.3%.

[0036] Comparative Example 1

[0037] The initial manganese slag leachate has a pH of 4.5, a manganese ion content of 13.89 g / l, a magnesium ion content of 14.13 g / l, and an ammonia nitrogen content of 6.27 g / l. 100 ml of manganese slag leachate is added to a beaker without adding manganese carbonate; 2.96 g of sodium carbonate is added, the pH is adjusted to 7.5, and the magnetic reaction is carried out for 4 hours in a sealed environment at 40°C, the manganese ion content drops to 1.51 g / l, the manganese recovery rate is 89.1%, the magnesium ion content is 13.62 / l, and the filter residue component is mainly manganese carbonate. 10.01 g of sodium dihydrogen phosphate is added to the filtrate, the pH is adjusted to 9.3, and the reaction is carried out for 17 minutes. The filter residue obtained after filtration is mainly magnesium ammonium phosphate. After the reaction, the manganese ion content is 0.57 g / l, the magnesium ion content is 1.52 g / l, and the magnesium recovery rate is 88.8%.

[0038] Comparative Example 2

[0039] The pH value of the initial manganese slag percolate is 4.5, the manganese ion content is 13.89 g / l, the magnesium ion content is 14.13 g / l, and the ammonia nitrogen content is 6.27 g / l. 100 ml of the manganese slag percolate is added to a beaker without adding manganese carbonate; 2.96 g of sodium carbonate is added, and the pH value is adjusted to 6.9. Under a sealed environment at 40° C., the magnetic reaction is carried out for 30 minutes, and the manganese ion content is reduced to 3.5 g / l, and the manganese recovery rate is 83.4%. The magnesium ion content is 13.65 / l, and the filter residue component is mainly manganese carbonate. 10.01 g of sodium dihydrogen phosphate is added to the filtrate, and the pH value is adjusted to 8. The reaction is carried out for 17 minutes. The filter residue obtained after filtration is mainly magnesium ammonium phosphate. After the reaction, the manganese ion content is 1.5 g / l, the magnesium ion content is 4.7 g / l, and the magnesium recovery rate is 65.5%.

[0040] Comparative Example 3

[0041] The pH value of the initial manganese slag percolate is 4.5, the manganese ion content is 13.89 g / l, the magnesium ion content is 14.13 g / l, and the ammonia nitrogen content is 6.27 g / l. 100 ml of the manganese slag percolate is added to a beaker without adding manganese carbonate; 2.96 g of sodium carbonate is added, and the pH value is adjusted to 8. Under a sealed environment at 40° C., the magnetic reaction is performed for 4 hours, and the manganese ion content is reduced to 1.3 g / l, the manganese recovery rate is 90.6%, and the magnesium ion content is 8.57 g / l. The filter residue components are mainly manganese carbonate and magnesium carbonate. Manganese carbonate and magnesium carbonate are difficult to separate and cannot be returned to the electrolytic cell as raw materials for electrolytic manganese for reuse. 5.3 g of sodium dihydrogen phosphate is added to the filtrate, the pH value is adjusted to 8, and the reaction is performed for 17 minutes. The filter residue obtained after filtration is mainly magnesium ammonium phosphate. After the reaction, the manganese ion content is 1.5 g / l, the magnesium ion content is 4.53 g / l, and the magnesium recovery rate is 47.1%.

Claims

1. A method for selective mineralization and cascade recovery of valuable components in manganese slag leachate, characterized in that: The steps include: Step (1) Add 0.02-3.5g of sodium carbonate and 0.01-2.5g of 400-800 mesh manganese carbonate to 100ml of manganese slag filtrate; add sodium carbonate and manganese carbonate to the manganese slag filtrate, and use a pH adjuster (sodium hydroxide, etc.) to adjust the pH to 7-7.5, stir magnetically at 40-50°C for 4-5h to produce manganese carbonate precipitation, filter, and recover the precipitated slag and filtrate after solid-liquid separation; Step (2) Magnesium ions and ammonia nitrogen components are also present in the filtrate. Sodium dihydrogen phosphate is added in a ratio of 0.2-12 g of sodium dihydrogen phosphate per 100 ml, the pH is adjusted to between 9.5 and 10, and magnetic stirring is performed for 15-30 minutes to produce a stable struvite precipitate.

2. The method for selective mineralization and cascade recovery of valuable components in manganese slag leachate according to claim 1, characterized in that: The main component of the precipitated slag obtained in step (1) is manganese carbonate, which can be used for the next step of smelting, or the precipitated slag can be ground to 400-800 mesh and directly used as the raw material for the precipitation in the crystal nucleus induction step 1.

3. The method for selective mineralization and cascade recovery of valuable components in manganese slag leachate according to claim 1, characterized in that: When the manganese ion concentration in the manganese slag leachate is less than or equal to 0.5g / l, sodium carbonate and manganese carbonate are added in a ratio of 0.02-0.5g sodium carbonate and 0.01-0.05g 400-800 mesh manganese carbonate to 100ml manganese slag leachate.

4. The method for selective mineralization and cascade recovery of valuable components in manganese slag leachate according to claim 1, characterized in that: When the manganese ion concentration in the manganese slag leachate is 10-15 g / l, sodium carbonate and manganese carbonate are added in a ratio of 2-3.5 g sodium carbonate and 1-2.5 g 400-800 mesh manganese carbonate to 100 ml manganese slag leachate.

5. The method for selective mineralization and cascade recovery of valuable components in manganese slag leachate according to claim 1, characterized in that: When the magnesium ion content in the manganese slag leachate is less than or equal to 0.5 g / l and the ammonia nitrogen content is less than or equal to 0.5 g / l, in step (2), sodium dihydrogen phosphate is added at a ratio of 0.2-1 g of sodium dihydrogen phosphate to 100 ml of liquid.

6. The method for selective mineralization and cascade recovery of valuable components in manganese slag leachate according to claim 1, characterized in that: When the magnesium ion content in the manganese slag leachate is greater than or equal to 5 g / l and the ammonia nitrogen content is less than or equal to 5 g / l, in step (2), sodium dihydrogen phosphate is added at a ratio of 7-12 g of sodium dihydrogen phosphate to 100 ml of liquid.

7. The method for selective mineralization and cascade recovery of valuable components in manganese slag leachate according to claim 1, characterized in that: The struvite precipitate obtained in step (2) is roasted to obtain roasted slag, the main component of which is magnesium phosphate.