Silicon-aluminum target material and preparation method thereof
By using the special protective design of the rotary spray back tube and the special particle size powder in the plasma spraying process, the problem of low density and deposition rate of silicon and aluminum targets is solved, and high-density and crack-free silicon and aluminum target preparation is achieved. Improved production efficiency and quality.
Patent Information
- Application Number
- CN202411196104.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The silicon-aluminum targets prepared by plasma spraying process have low density and low deposition rate, and are prone to cracks on the surface due to concentrated stress, making it difficult to meet the standards of industrial mass production.
The special protective design of the rotary spray back tube and the selection of powder raw materials with special particle sizes are set, and NiAl coating and heat-resistant tape are wound to form high-density, silicon-aluminum targets without obvious cracks are formed through plasma spraying.
The density and deposition rate of silicon-aluminum targets are improved, stress concentration problems are avoided, and production efficiency and product quality are improved.
Smart Images

Figure BDA0005016451700000061 
Figure HDA0005016451710000011
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal processing, and in particular to a silicon-aluminum target material and a preparation method thereof. Background Art
[0002] The plasma spraying process for preparing silicon aluminum targets is not limited by size and space, and can prepare target products of any size according to actual needs. In theory, it can well replace the existing powder pressing and sintering process. However, the target products prepared by this process have problems such as low density and low deposition rate. The surface of the product, especially the end position, is prone to cracks due to stress concentration. The controlled factors are complex, and the efficiency and quality of product production are difficult to meet the standard requirements of industrial mass production. Summary of the invention
[0003] Based on the defects of the prior art, the purpose of the present invention is to provide a method for preparing a silicon-aluminum target material. The method still adopts a plasma spraying process, but when preparing the product, through the special protection design of the rotary spraying back tube and the selection of powder raw materials with a special particle size, the prepared product can have a high deposition rate and high production efficiency on the basis of high density and no obvious cracks.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is:
[0005] A method for preparing a silicon-aluminum target material comprises the following steps:
[0006] (1) providing a rotary spray back tube, performing a sandblasting process on the rotary spray back tube, and then providing a NiAl coating on a spraying portion of the rotary spray back tube by arc spraying;
[0007] (2) wrapping the two ends of the rotary sprayed back tube provided with the NiAl coating with a heat-resistant tape, and then covering the wrapping of the heat-resistant tape with a sheath;
[0008] (3) placing the mixed powder into a plasma sprayer, and then plasma spraying the mixed powder on the rotary spray backing tube to form a silicon-aluminum target; the mixed powder includes silicon powder and aluminum powder, the mass ratio of the silicon powder to the aluminum powder is (91:9) to (95:5), the particle size of the silicon powder is 45 to 150 μm, and the mass content of the silicon powder with a particle size of 75 to 150 μm accounts for 30 to 50 wt%;
[0009] (4) After the silicon-aluminum target material is sprayed to a predetermined thickness, it is cooled, thereby completing the preparation of the silicon-aluminum target material.
[0010] The plasma spraying process does not need to consider the size of the product when preparing the target material. However, compared with the traditional powder hot pressing and sintering process, the existing plasma spraying process is mostly implemented in the laboratory in a low-power, low-yield mode (that is, only the quality of the target material is considered, and the actual target material production efficiency is not considered). If batch production is carried out according to factory standards, the silicon aluminum target material prepared by the plasma spraying process has a low density and a low deposition rate. It is difficult to meet commercial standards in terms of production efficiency and the quality of the target material. At the same time, during the plasma spraying process, due to stress concentration problems, cracks often appear on the surface of the produced silicon aluminum target material, and the product cannot meet the use requirements.
[0011] To this end, in the technical solution of the present invention, without considering setting additional processes or regulating parameters, firstly, powder with a special size distribution is selected as the raw material for plasma spraying, and then a NiAl coating with a primer effect is pre-set on the deposited rotary spray back tube, and a heat-resistant tape is used for winding treatment at both ends, and finally the treated part is covered with a sheath. During the plasma spraying process, the powder particles can be fully melted and deposited on the back tube, with a high deposition rate and a high density of the deposited particles. At the same time, the wound heat-resistant tape plays a transitional role between the NiAl coating and the non-coated area. The powder particles will not cause a stress concentration effect during deposition, so that cracks appear at both ends of the formed target material and extend to the central part, and no obvious cracks appear on the surface of the prepared target material product.
[0012] Preferably, the NiAl coating has a thickness of 0.5-1.3 mm.
[0013] By providing a NiAl coating with a primer function on the rotary spraying back tube, the particles generated by plasma spraying can be uniformly deposited on the back tube with a high deposition density. The above thickness can make the product have a higher density and uniformity without affecting the production efficiency.
[0014] Preferably, the heat-resistant tape is Teflon tape, more preferably 3J76B Teflon tape.
[0015] More preferably, when the heat-resistant tape is wound around one end of the rotary sprayed backing tube provided with a NiAl coating, the tape has a width of 12 to 14 mm and a length of 415 to 420 mm, and a thickness of 0.1 to 0.3 mm after winding.
[0016] Preferably, the sheath is a stainless steel annular sheath with a thickness of 1.5 to 2.5 mm. When the sheath is covered with a heat-resistant tape, the parallel distance between the heat-resistant tape and the uncovered area of the rotary spray back tube is 3 to 6 mm.
[0017] By setting up the heat-resistant tape and the sheath, it is possible to avoid the stress concentration problem caused by spraying the plasma sprayed deposited layer at the junction of the NiAl layer and the non-NiAl layer area, thereby preventing cracks from occurring in this area and extending to the central part, thereby effectively ensuring the quality of the target material obtained by plasma spraying.
[0018] Preferably, the purity of the silicon powder is ≥3N, and the purity of the aluminum powder is ≥2N8;
[0019] More preferably, the particle size of the aluminum powder is 50 to 120 μm.
[0020] Preferably, in step (1), the outer diameter of the rotary spray backing tube is 120-150 mm, and the length is 3000-3500 mm.
[0021] Preferably, in the step (3), the working power during the plasma spraying is 30-35 kW, the moving speed of the spray gun used in the plasma spraying is 35-45 mm / min, the spraying distance is 100-150 mm, the rotation speed of the rotary spraying back tube is 200-300 rpm, the powder feeding amount of the mixed powder is 190-200 g / min, and the powder feeding gas flow rate is 3.5-4.5 nL / min.
[0022] More preferably, the spray gun is provided with a plasma generating pipeline, in which a mixed gas is provided, the mixed gas comprises argon and hydrogen, the argon flow rate is 2600-2700 nL / h, and the hydrogen flow rate is 450-500 nL / h.
[0023] In the argon and hydrogen mixed gas connected to the spray gun, the argon generates plasma under the action of the electric field, and the hydrogen plays a combustion-supporting role, and the titanium dioxide powder sent to the spray gun is deposited under the above-mentioned action.
[0024] Another object of the present invention is to provide a silicon-aluminum target material prepared by the method for preparing the silicon-aluminum target material.
[0025] Preferably, the thickness of the silicon-aluminum target is ≥9 mm.
[0026] Preferably, the density of the silicon aluminum target is 2 to 2.5 g / cm 3 , resistivity is 0.015~0.020Ω / cm, and deposition rate is 30~35%.
[0027] The beneficial effect of the present invention is that the present invention provides a method for preparing a silicon aluminum target material, which adopts a plasma spraying process. When preparing the product, through the special protection design of the rotary spraying back tube and the selection of powder raw materials with a special particle size, the prepared product can have a high deposition rate and high production efficiency on the basis of high density and no obvious cracks.
[0028] Instruction Manual
[0029] Figure 1 The figure is a schematic diagram of the arrangement of the rotary spraying back tube according to the present invention. DETAILED DESCRIPTION
[0030] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.
[0031] Example 1
[0032] An embodiment of a silicon-aluminum target material and a method for preparing the same according to the present invention comprises the following steps:
[0033] (1) a rotary spray back tube with an outer diameter of 133 mm and a length of 3191 mm is provided, the rotary spray back tube is subjected to sandblasting, and then a NiAl coating with a thickness of 1 mm is provided on the spraying portion of the rotary spray back tube by arc spraying as a primer;
[0034] (2) The two ends of the rotary spray back tube with NiAl coating are wrapped with heat-resistant tape, and then the wrapped parts of the heat-resistant tape (also called high-temperature tape) are covered with a sheath, and the length of the sheath covering the base layer (that is, the parallel distance between the heat-resistant tape and the uncovered area of the rotary spray back tube) is 5 mm; Figure 1 As shown; the heat-resistant tape is 3J76B Teflon tape, and when winding, the winding width is 13mm, the length is 417.62mm, and the winding thickness is 0.2mm; the sheath is a 304 stainless steel ring sheath with a thickness of 2mm;
[0035] (3) 3N silicon powder and 2N8 aluminum powder were placed in a mixer at a mass ratio of 93:7 and mixed for 6 hours. After drying at 60°C for 6 hours, the resulting mixed powder was placed in an SN-DQPT-4600L plasma sprayer, and then plasma sprayed on a rotary spray backing tube to form a silicon-aluminum target; the silicon powder was sieved and had a particle size of 45 to 150 μm, of which the mass content of silicon powder with a particle size of 75 to 150 μm accounted for 48 wt%, and the average particle size of the silicon powder in this part was 110 μm. The particle size of the remaining silicon powder was 45 to 75 μm, and the average particle size of the silicon powder in this part was 60 μm; the particle size of the aluminum powder was 50 to 120 μm, and the average particle size was 85 μm;
[0036] During the plasma spraying, the power is set to 33.4kW, the spray gun moves back and forth, the rotary spray back tube rotates from the axis, the movement speed of the spray gun is 42mm / min, the spraying distance is 140mm, the rotation speed of the rotary spray back tube is 240rpm, the powder feeding amount of the mixed powder is 190g / min, the powder feeding gas flow rate is 4nL / min, the spray gun is provided with a plasma generating pipeline, and a mixed gas is provided in the plasma generating pipeline, the mixed gas includes argon and hydrogen, the argon flow rate is 2600nL / h, and the hydrogen flow rate is 500nL / h;
[0037] (4) After the silicon-aluminum target material is sprayed to a predetermined thickness of 9.1 mm, it is cooled, and the preparation of the silicon-aluminum target material is completed.
[0038] Example 2
[0039] The embodiment of a silicon-aluminum target material and a preparation method thereof described in the present invention is different from Example 1 only in that the thickness of the NiAl coating is 1.2 mm; heat-resistant tape is used to wrap the two ends of the rotary spraying backing tube provided with the NiAl coating, and then a sheath is used to cover the wrapped part of the heat-resistant tape, and the sheath covers the base layer for a length of 6 mm; during the plasma spraying, the power is set to 34 kW; the predetermined thickness of the silicon-aluminum target material deposition is 9.2 mm.
[0040] Example 3
[0041] The embodiment of a silicon-aluminum target material and a preparation method thereof described in the present invention is different from Embodiment 1 only in that the mass ratio of silicon powder to aluminum powder in the mixed powder is 94:6.
[0042] Example 4
[0043] The embodiment of a silicon-aluminum target material and a preparation method thereof described in the present invention differs from Example 1 only in that the silicon powder is sifted and has a particle size of 45 to 150 μm, wherein the mass content of silicon powder with a particle size of 75 to 150 μm accounts for 45wt%, and the average particle size of this part of silicon powder is 120 μm, and the particle size of the remaining silicon powder is 45 to 75 μm, and the average particle size of this part of silicon powder is 50 μm; the particle size of the aluminum powder is 50 to 120 μm, and the average particle size is 90 μm.
[0044] Example 5
[0045] The embodiment of a silicon-aluminum target material and a preparation method thereof described in the present invention differs from Example 1 only in that the silicon powder is sifted and has a particle size of 45 to 150 μm, wherein the mass content of silicon powder with a particle size of 75 to 150 μm accounts for 42wt%, and the average particle size of this part of silicon powder is 130 μm, and the particle size of the remaining silicon powder is 45 to 75 μm, and the average particle size of this part of silicon powder is 55 μm; the particle size of the aluminum powder is 50 to 120 μm, and the average particle size is 100 μm.
[0046] Comparative Example 1
[0047] A silicon aluminum target material and a preparation method thereof, which differs from Example 1 only in that the rotary spraying back tube is not provided with heat-resistant tape winding and sheath covering after the NiAl coating is provided, and the predetermined thickness of the silicon aluminum target material deposition is 9.4 mm.
[0048] Comparative Example 2
[0049] A silicon aluminum target material and a preparation method thereof, which differs from Example 1 only in that after the rotary spraying back tube is provided with a NiAl coating and wrapped with a heat-resistant tape, a sheath covering is no longer provided.
[0050] Comparative Example 3
[0051] A silicon-aluminum target material and a preparation method thereof, which differ from Example 1 only in that the silicon powder is sifted and has a particle size of 20 to 120 μm, wherein the mass content of silicon powder with a particle size of 50 to 120 μm accounts for 48wt%, and the average particle size of this part of silicon powder is 90 μm, and the particle size of the remaining silicon powder is 20 to 50 μm, and the average particle size of this part of silicon powder is 30 μm; the predetermined thickness of the silicon-aluminum target material deposition is 9.4 mm.
[0052] Comparative Example 4
[0053] A silicon-aluminum target material and a preparation method thereof, which differs from Example 1 only in that the silicon powder is sifted and has a particle size of 70 to 180 μm, wherein the mass content of silicon powder with a particle size of 120 to 180 μm accounts for 48wt%, and the average particle size of this part of silicon powder is 150 μm, and the particle size of the remaining silicon powder is 70 to 120 μm, and the average particle size of this part of silicon powder is 85 μm.
[0054] Effect Example 1
[0055] In order to verify the effect of the silicon aluminum target material prepared by the preparation method of the present invention, the density (Archimedes method), average resistivity (directly tested by a four-probe resistivity meter), and deposition rate (directly measured by weight) tests were performed on the products of each embodiment and comparative example, and at the same time, whether cracks appeared on the surface of the product (typically, whether cracks extending toward the center appeared at both ends of the target material), and the test results are statistically summarized in Table 1.
[0056] Table 1
[0057]
[0058] It can be seen from Table 1 that the silicon-aluminum target prepared by the preparation method of the present invention has a high quality and the density of the target can reach 2.220 g / cm 3 The average resistivity can be maintained within the range of 0.015-0.016Ω / cm, the deposition rate reaches more than 32%, and there is no obvious crack defect in the appearance.
[0059] It can be seen from Example 1, Examples 4 to 5 and Comparative Examples 3 to 4 that the size of the powder particles used in plasma spraying has a great influence on the performance of the prepared product, especially for silicon powder, which accounts for a large proportion. When the silicon powder particles used are smaller or larger, the particles will not be fully uniform during melting and deposition, and the deposition rate of the prepared target product and the density of the obtained product will be affected. Although the density of the product in Comparative Example 3 is relatively high, the deposition success rate is low and the deposition rate is relatively low because the silicon powder particles used are too large. The silicon powder used in the preparation of the product in Comparative Example 4 is relatively small, and not only the deposition rate is low, but the density of the obtained target product is also lower than expected.
[0060] According to Example 1, Comparative Examples 1 and 2, it can be seen that when the rotary spraying backing tube is not set up at all and the mixed powder defined in the present invention is used for plasma spraying, uneven force and stress concentration are likely to occur when the particles are deposited on the primer coating and non-priming coating at both ends, so the prepared product cracks from both ends and extends to the central part; on this basis, the method described in Comparative Example 2 sets a heat-resistant tape to carry out an incorporation treatment on the transition area between the primer coating and the non-priming coating, but this will cause the particles to be deposited in this area and completely cover the heat-resistant tape, and it still cannot relieve stress in the subsequent deposition process, and the obtained target product still has cracks. Only the method of Example 1 in which heat-resistant tape winding and sheath covering are set up at the same time can effectively avoid the problem of stress concentration in the product during the entire process of particle deposition, so the obtained target product has no cracks.
[0061] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a silicon-aluminum target material, It is characterized in that The following steps are involved: (1) providing a rotary spray back tube, performing a sandblasting process on the rotary spray back tube, and then providing a NiAl coating on a spraying portion of the rotary spray back tube by arc spraying; (2) wrapping the two ends of the rotary sprayed back tube provided with the NiAl coating with a heat-resistant tape, and then covering the wrapping of the heat-resistant tape with a sheath; (3) placing the mixed powder into a plasma sprayer, and then plasma spraying the mixed powder on the rotary spray backing tube to form a silicon-aluminum target; the mixed powder includes silicon powder and aluminum powder, the mass ratio of the silicon powder to the aluminum powder is (91:9) to (95:5), the particle size of the silicon powder is 45 to 150 μm, and the mass content of the silicon powder with a particle size of 75 to 150 μm accounts for 30 to 50 wt%; (4) After the silicon-aluminum target material is sprayed to a predetermined thickness, it is cooled, thereby completing the preparation of the silicon-aluminum target material.
2. The method for preparing the silicon aluminum target according to claim 1, It is characterized in that The thickness of the NiAl coating is 0.5-1.3 mm.
3. The method for preparing the silicon aluminum target according to claim 1, It is characterized in that The particle size of the aluminum powder is 50 to 120 μm.
4. The method for preparing the silicon aluminum target according to claim 1, It is characterized in that In the step (3), the working power during the plasma spraying is 30-35 kW, the moving speed of the spray gun used in the plasma spraying is 35-45 mm / min, the spraying distance is 100-150 mm, the rotation speed of the rotary spraying back tube is 200-300 rpm, the powder feeding amount of the mixed powder is 190-200 g / min, and the powder feeding gas flow rate is 3.5-4.5 nL / min.
5. The silicon-aluminum target material prepared by the method for preparing the silicon-aluminum target material according to any one of claims 1 to 4.
6. The silicon aluminum target material according to claim 5, It is characterized in that The thickness of the silicon aluminum target material is ≥9 mm.
7. The silicon aluminum target material according to claim 5, It is characterized in that The density of the silicon aluminum target is 2 to 2.5 g / cm 3 , resistivity is 0.015~0.020Ω / cm, and deposition rate is 30~35%.
Citation Information
Patent Citations
Preparation method of high-compactness aluminum-silicon rotary target material
CN108707870A
Sandblast protector of rotatory target of large -scale spraying
CN207480409U
Method of spraying electrically conducting metal-carbon multilayer coating on tape substrate made of nonwoven fibrous material
RU2677551C1
Cited By
Aluminum-scandium alloy target material and preparation method thereof
CN121087432A