Titanium dioxide target material and preparation method thereof
The plasma spraying process with controlled temperature regulation and cooling systems addresses the limitations of existing methods, producing high-density, crack-free titanium dioxide targets with improved deposition rates and uniformity.
Patent Information
- Application Number
- CN202411196105.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
AI Technical Summary
Existing methods for preparing titanium dioxide targets, such as hot pressing and sintering, are limited in size and complexity, while plasma spraying results in low density, low deposition rate, and thermal stress-induced cracking due to titanium dioxide's low thermal expansion coefficient.
A plasma spraying process with regulated process parameters and a cooling system to control real-time surface temperature, using a rotary spray back tube with coolant and cooling air pipes to maintain the target material's temperature within specific ranges, ensuring high density and deposition rate without cracks.
The method produces titanium dioxide targets with high density and deposition rate, achieving large thickness without surface cracks, improving product quality and process efficiency.
Smart Images

Figure BDA0005016451950000071 
Figure HDA0005016451970000011
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal processing, and in particular to a titanium dioxide target material and a preparation method thereof. Background Art
[0002] Titanium dioxide targets are widely used in the preparation of Low-E glass and anti-reflective glass due to their excellent light transmittance, high refractive index and high corrosion resistance. At present, the main preparation method of titanium dioxide targets is hot pressing and sintering. However, this method has some limitations on the size of the prepared products and cannot produce products with higher thickness. At the same time, this type of process generally requires multiple pretreatments, pressing and sintering of powder raw materials to obtain the final product. The preparation process is very complicated and cannot be mass-produced.
[0003] The plasma spraying process for preparing oxide targets is not limited by size and space. In theory, it can replace the traditional hot pressing and sintering process to produce titanium dioxide target products of ultra-large volume and thickness. However, the products prepared by this technology have the problems of low density and low deposition rate. At the same time, due to the low thermal expansion coefficient of titanium dioxide and the difficulty in heat dissipation, the thermal stress accumulated during the production process will make the prepared products prone to surface cracks, and the quality is far inferior to the products prepared by traditional processes. Summary of the invention
[0004] Based on the defects of the prior art, the purpose of the present invention is to provide a method for preparing a titanium dioxide target material, which prepares a target material product by a titanium dioxide powder plasma spraying process. At the same time, during the product preparation process, the process parameters are regulated and a cooling system is set to control the real-time surface temperature of the target material, so that the prepared product still has the characteristics of high density and high deposition rate at a large thickness, and there are no obvious cracks on the product surface.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for preparing a titanium dioxide target material comprises the following steps:
[0007] (1) a rotary spray back tube is provided, and the rotary spray back tube is subjected to sandblasting and arc spraying treatment; the rotary spray back tube is in the shape of a long tube, and a core shaft is provided inside the tube; a coolant is provided inside the core shaft; and the temperature of the coolant is 50 to 60° C.;
[0008] (2) placing titanium dioxide powder with an average particle size of 45 to 120 μm into a plasma sprayer, and then plasma spraying it on a rotary spray backing tube; at the same time, a cooling air pipe is set to purge the spray backing tube, and the temperature of the titanium dioxide target obtained by spraying is controlled to be 100 to 130° C.; the vertical distance between the spray gun used for the plasma spraying and the rotary spray backing tube is 160 to 190 mm;
[0009] (3) After the titanium dioxide target material is sprayed to a predetermined thickness, the plasma spraying is stopped and the rotary spraying backing tube is purged for 140 to 150 minutes, and the coolant temperature of the core shaft of the rotary spraying backing tube is set to be lowered to 20 to 30° C.;
[0010] (4) After the titanium dioxide target material is cooled to room temperature, the preparation of the titanium dioxide target material is completed.
[0011] The plasma spraying process does not need to consider the size of the product when preparing the target material, so in theory, it is possible to produce target materials of extremely great thickness. However, since plasma spraying mainly deposits oxide particles on a rotary spraying backing tube in a spraying manner to prepare the target material, it is easy for the target material to have a low relative density and a low deposition rate. For the titanium dioxide target material described in the technical solution of the present invention, since it has a low thermal expansion coefficient and is not easy to dissipate heat, it is easy to accumulate thermal stress during the plasma spraying process. Once the target material is deposited too thick, it is easy to crack, and the product quality cannot be guaranteed. To this end, in the technical solution of the present invention, when titanium dioxide powder is plasma sprayed, a coolant with a specific temperature is set in the rotary spraying back tube. At the same time, during the plasma spraying process, the rotary spraying back tube is purged to control the surface temperature of the titanium dioxide target deposited on the back tube to always remain in the range of 100-130°C, which can not only effectively promote the combination of the titanium dioxide target and the rotary spraying back tube during deposition, but also avoid the accumulation of thermal stress during plasma spraying; when the plasma spraying is completed and purged and cooled, the temperature of the coolant is synchronously controlled to drop to 20-30°C, which can effectively avoid overheating of the internal and external temperature difference of the titanium dioxide target, and ensure that the target will not crack during the entire process.
[0012] At the same time, the inventors noticed that the powder size and spraying distance used in the plasma spraying process will have a great impact on the quality of the prepared titanium dioxide target. If not properly controlled, not only will the product fail to guarantee sufficient density and deposition rate, but it may even have appearance cracks, so it needs to be strictly limited.
[0013] Preferably, in step (1), the outer diameter of the rotary spray backing tube is 120-150 mm, and the length is 300-500 mm.
[0014] Preferably, in the step (1), the thickness of the sprayed layer on the rotary sprayed back tube after the arc spraying treatment is 0.5 to 0.7 mm.
[0015] Pre-processing the rotary spray backing tube with sandblasting and arc spraying can improve the tightness of the plasma sprayed titanium dioxide powder and the rotary spray backing tube in the process of forming a target material, so that the prepared product has higher density and uniformity.
[0016] Preferably, in step (2), the working current during plasma spraying is 450-510A, the working voltage is 55-64V, the movement speed of the spray gun is 35-45mm / min, the rotation speed of the rotary spray back tube is 230-260rpm, the powder feeding amount is 92-96g / min, and the powder feeding gas flow rate is 2.4-2.9nL / min.
[0017] More preferably, the spray gun is provided with a plasma generating pipeline, in which a mixed gas is provided, the mixed gas comprises argon and hydrogen, the argon flow rate is 2200-2400 nL / h, and the hydrogen flow rate is 300-350 nL / h.
[0018] In the argon and hydrogen mixed gas connected to the spray gun, the argon generates plasma under the action of the electric field, and the hydrogen plays a combustion-supporting role, and the titanium dioxide powder sent to the spray gun is deposited under the above-mentioned action.
[0019] Preferably, in the step (2), a dust removal device is provided during the plasma spraying to perform dust removal, and the frequency of the dust removal device is 30 to 35 Hz.
[0020] The dust removal device can be used to remove the molten powder deposited on the target material in time to avoid the situation where the local temperature of the target material is too high and thermal stress is generated.
[0021] Preferably, in step (2), the number of cooling air pipes is 2, the air jets of the cooling air pipes are parallel to the spray gun muzzle of the plasma spraying machine and perpendicular to the axial direction of the rotary spraying back tube, and the vertical distance from the rotary spraying back tube is 20 to 30 mm.
[0022] More preferably, the interval between the two cooling air pipes is 100-200 mm, the inner diameter of the cooling air pipe is 6-8 mm, the outer diameter is 8-10 mm, the length is 150-200 mm, and the purge pressure is 3-4 kg.
[0023] More preferably, the purge gas of the cooling air pipe is at least one of air and inert atmosphere.
[0024] By setting the above-mentioned preferred cooling air pipe, the surface temperature of the target material obtained by plasma spraying can be effectively and real-time reduced, while ensuring the uniformity and high deposition of plasma spraying, and the quality of the obtained titanium dioxide target material is better.
[0025] Preferably, when the cooling air pipe is purging the titanium dioxide target in step (3), the rotation speed of the rotary spraying backing tube is 50 to 80 rpm.
[0026] During the cooling process of the titanium dioxide target, in order to avoid the cooling effect being concentrated only on the bottom of the target and to ensure the cooling uniformity of the target, it is necessary to reduce the rotation speed of the back tube, thereby avoiding cracks in the target due to local temperature unevenness during the cooling process.
[0027] Preferably, the purity of the titanium dioxide powder is 99.95-99.99%, and the bulk density is 1.5-2 g / cm 3 .
[0028] Another object of the present invention is to provide a titanium dioxide target material prepared by the method for preparing the titanium dioxide target material.
[0029] Preferably, the thickness of the titanium dioxide target is ≥10 mm.
[0030] The method for preparing the titanium dioxide target material of the present invention prepares the target material by using a plasma spraying process. When the process is carried out, specific spraying parameters are selected and a cooling device and a program are used in combination, so that the product can still have high density and high deposition rate in the case of a large thickness; the product surface has no obvious cracks and has high overall quality.
[0031] Preferably, the density of the titanium dioxide target is 4 to 4.2 g / cm 3 , resistivity is 0.12~0.16Ω / cm, and deposition rate is 54~56%.
[0032] The beneficial effect of the present invention is that the present invention provides a method for preparing a titanium dioxide target material, which prepares a target material product by a titanium dioxide powder plasma spraying process, and at the same time, during the product preparation process, the process parameters are regulated and a cooling system is set to control the real-time surface temperature of the target material, so that the prepared product still has the characteristics of high density and high deposition rate at a large thickness, and there are no obvious cracks on the product surface.
[0033] Instruction Manual
[0034] Figure 1 The figure is a schematic diagram of the process of preparing the titanium dioxide target material of the present invention by plasma spraying. DETAILED DESCRIPTION
[0035] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.
[0036] Example 1
[0037] An embodiment of a titanium dioxide target material and a preparation method thereof according to the present invention comprises the following steps:
[0038] (1) A stainless steel rotary spray back tube with an outer diameter of 133 mm and a length of 400 mm, which has been pre-cleaned and polished, is provided, and the rotary spray back tube is sandblasted and arc sprayed, and the thickness of the spray layer is 0.5 mm; the rotary spray back tube is a long tube, and a core shaft is provided inside the tube; cooling water is provided inside the core shaft; the setting temperature of the cooling liquid is 50° C.;
[0039] (2) The average particle size is 60 μm, the purity is 99.99%, and the bulk density is 1.6 g / cm 3 The titanium dioxide powder is placed in the SN-DQPT-4600L plasma sprayer, and then the current is set to 510A, the voltage is 63V, the powder feeding amount is 96g / min, the powder feeding air (i.e., carrier gas) flow rate is 2.6nL / min, the spray gun moves back and forth, the rotary spray back tube rotates about the axis, the movement rate of the spray gun is 40mm / min, the rotation speed of the rotary spray back tube is 240rpm, and plasma spraying is performed on the rotary spray back tube; at the same time, a cooling air pipe is set to purge the spray back tube , controlling the temperature of the titanium dioxide target obtained by spraying to be 100-130°C; at the same time, a dust removal device is also provided for synchronous dust removal treatment, the frequency of the dust removal device is 30Hz, and the vertical distance between the spray gun used for plasma spraying and the rotary spray back tube is 190mm; the spray gun is provided with a plasma generating pipeline, and a mixed gas is provided in the plasma generating pipeline, the mixed gas includes argon and hydrogen, the argon flow rate is 2400nL / h, and the hydrogen flow rate is 350nL / h;
[0040] like Figure 1 As shown, the number of the cooling air pipes is 2, and the air jets of the cooling air pipes are parallel to the spray gun muzzle of the plasma spraying machine and perpendicular to the axial direction of the rotary spraying back tube, and the vertical distance from the rotary spraying back tube is 25 mm.
[0041] The interval between the two cooling air pipes is 150 mm, the inner diameter of the cooling air pipe is 6 mm, the outer diameter is 10 mm, the length is 180 mm, the purge pressure is 3 kg, and the purge gas of the cooling air pipe is compressed air;
[0042] (3) After the titanium dioxide target material is sprayed to a predetermined thickness of 10 mm, the plasma spraying is stopped and the rotary spraying backing tube is purged for 140 min to cool it down. At the same time, the rotation speed of the rotary spraying backing tube is reduced to 80 rpm, and the cooling water temperature of the core shaft of the rotary spraying backing tube is set to be reduced to 30° C.;
[0043] (4) After the titanium dioxide target material is cooled to room temperature, the preparation of the titanium dioxide target material is completed.
[0044] Example 2
[0045] The embodiment of a titanium dioxide target material and a preparation method thereof according to the present invention, the preparation method, which differs from the embodiment 1 only in that it comprises the following steps:
[0046] (1) A stainless steel rotary spray back tube with an outer diameter of 133 mm and a length of 400 mm, which has been pre-cleaned and polished, is provided, and the rotary spray back tube is sandblasted and arc sprayed, and the thickness of the spray layer is 0.5 mm; the rotary spray back tube is a long tube, and a core shaft is provided inside the tube; cooling water is provided inside the core shaft; the setting temperature of the cooling liquid is 50° C.;
[0047] (2) The average particle size is 60 μm, the purity is 99.99%, and the bulk density is 1.8 g / cm 3 The titanium dioxide powder is placed in the SN-DQPT-4600L plasma sprayer, and then the current is set to 500A, the voltage is set to 60V, the powder feeding amount is set to 95g / min, the powder feeding air (i.e., carrier gas) flow rate is set to 2.8nL / min, the movement rate of the spray gun is set to 40mm / min, the rotation speed of the rotary spraying back tube is set to 240rpm, and plasma spraying is performed on the rotary spraying back tube; at the same time, a cooling air pipe is set to purge the spraying back tube, and the temperature of the titanium dioxide target obtained by spraying is controlled to be 100-130°C; at the same time, a dust removal device is also provided for synchronous dust removal treatment, the frequency of the dust removal device is 30Hz, and the vertical distance between the spray gun used for plasma spraying and the rotary spraying back tube is 190mm; the spray gun is provided with a plasma generating pipeline, and a mixed gas is provided in the plasma generating pipeline, and the mixed gas includes argon and hydrogen, the argon flow rate is 2400nL / h, and the hydrogen flow rate is 350nL / h;
[0048] (3) After the titanium dioxide target material is sprayed to a predetermined thickness of 10 mm, the plasma spraying is stopped and the rotary spraying backing tube is purged for 140 min to cool it down. At the same time, the rotation speed of the rotary spraying backing tube is reduced to 80 rpm, and the cooling water temperature of the core shaft of the rotary spraying backing tube is set to be reduced to 30° C.;
[0049] (4) After the titanium dioxide target material is cooled to room temperature, the preparation of the titanium dioxide target material is completed.
[0050] Example 3
[0051] The embodiment of a titanium dioxide target material and a preparation method thereof described in the present invention is different from Embodiment 1 only in that the average particle size of the titanium dioxide powder is 85 μm.
[0052] Example 4
[0053] The embodiment of a titanium dioxide target material and a preparation method thereof described in the present invention is different from the embodiment 1 only in that the vertical distance between the spray gun used for the plasma spraying and the rotary spraying back tube is 180 mm.
[0054] Example 5
[0055] The embodiment of a titanium dioxide target material and a preparation method thereof described in the present invention is different from the embodiment 1 only in that the vertical distance between the spray gun used for the plasma spraying and the rotary spraying back tube is 160 mm.
[0056] Comparative Example 1
[0057] A titanium dioxide target material and a preparation method thereof, the difference from Example 1 is that the average particle size of the titanium dioxide powder is 35 μm.
[0058] Comparative Example 2
[0059] A titanium dioxide target material and a preparation method thereof, the difference from Example 1 is that the average particle size of the titanium dioxide powder is 135 μm.
[0060] Comparative Example 3
[0061] A titanium dioxide target material and a preparation method thereof, the only difference from Example 1 is that no cooling water is provided in the core shaft.
[0062] Comparative Example 4
[0063] A titanium dioxide target material and a preparation method thereof, the only difference from Example 1 is that during the plasma spraying process, no cooling air pipe is provided to purge the spraying back tube, thereby controlling the temperature of the titanium dioxide target material obtained by spraying to be 100-130°C, and only 50°C cooling water is provided in the core shaft for cooling, and after stopping the plasma spraying in step (3), only the rotation speed of the rotating spraying back tube and the temperature of the cooling water are reduced.
[0064] Comparative Example 5
[0065] A titanium dioxide target material and a preparation method thereof, which differs from Example 1 only in that the vertical distance between the spray gun used for plasma spraying and the rotary spraying back tube is 140 mm.
[0066] Comparative Example 6
[0067] A titanium dioxide target material and a preparation method thereof, the only difference from Example 1 is that the vertical distance between the spray gun used for plasma spraying and the rotary spraying back tube is 210 mm.
[0068] Effect Example 1
[0069] In order to verify the effect of the titanium dioxide target material prepared by the preparation method of the present invention, the density (Archimedes method), average resistivity (directly tested by a four-probe resistivity meter), and deposition rate (directly measured by weight) tests were performed on the products of each embodiment and comparative example, and at the same time, it was observed whether cracks appeared on the surface of the product (typically, "turtle back" cracks appeared on the surface). The test results are summarized in Table 1.
[0070] Table 1
[0071]
[0072]
[0073] It can be seen from Table 1 that the titanium dioxide target prepared by the preparation method of the present invention has high quality and the density of the target can reach 4.15 g / cm 3 The average resistivity can be maintained within the range of 0.12 to 0.15 Ω / cm, the deposition rate is above 50%, and there is no obvious crack defect in the appearance.
[0074] It can be seen from Example 1, Example 3 and Comparative Examples 1 to 2 that the particle size of the titanium dioxide powder used in plasma spraying has a great influence on the performance of the prepared product. When the particles are small, over-melting is likely to occur during plasma spraying, and the accumulated heat is difficult to disperse, resulting in not only a low deposition rate, but also huge thermal stress that causes obvious "turtle back" cracks to appear on the surface of the target material. On the other hand, the titanium dioxide powder particles used in the preparation of the product in Comparative Example 2 are too large. During the plasma spraying process, the powder solidifies before being deposited on the surface of the back tube, thereby forming a "nodule" on the surface of the prepared target material, which in turn results in a low density of the product, a low deposition rate, uneven composition, and obvious unevenness on the surface of the target material, resulting in poor overall quality.
[0075] According to Example 1, Examples 4 to 5 and Comparative Examples 5 to 6, it can be seen that during plasma spraying, the spray distance setting of the spray gun is very critical. If it is set too short, the powder cannot be completely melted during the spraying process, and the success rate of depositing on the back tube to form a target material is low, and the density and deposition rate of the target material are difficult to guarantee. At the same time, the cooling setting cannot be fully implemented, and the thermal stress generated during deposition cannot be eliminated in time, so the product also has surface cracks. If the distance is set too far, the sprayed powder solidifies before it is deposited on the back tube, and it is also difficult to guarantee the density and deposition rate of the titanium dioxide target material. Therefore, it needs to be specifically limited to the range of 160 to 190 mm.
[0076] According to the performance comparison of the products prepared in Example 1 and Comparative Examples 3 to 4, it can be seen that during the plasma spraying process, the coolant and the cooling air duct set on the rotary spray back tube core shaft can effectively remove the thermal stress accumulated in the target material during the deposition process, thereby ensuring that the product will not crack during the production process. The process of Comparative Example 3 does not have cooling water, and the temperature difference between the inside and outside of the target material is too large, thereby generating a stress difference, which ultimately leads to surface cracking; and the product of Comparative Example 4 does not have a cooling air duct for air sweeping treatment during preparation. As the thickness of the target material obtained by plasma spraying increases, the temperature of the target surface continues to rise to above 160°C, which ultimately leads to cracking of the target material due to thermal stress during the deposition process.
[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a titanium dioxide target, characterized in that: The following steps are involved: (1) a rotary spray back tube is provided, and the rotary spray back tube is subjected to sandblasting and arc spraying treatment; the rotary spray back tube is in the shape of a long tube, and a core shaft is provided inside the tube; a coolant is provided inside the core shaft; and the temperature of the coolant is 50 to 60° C.; (2) placing titanium dioxide powder with an average particle size of 45 to 120 μm into a plasma sprayer, and then plasma spraying it on a rotary spray backing tube; at the same time, a cooling air pipe is set to purge the spray backing tube, and the temperature of the titanium dioxide target obtained by spraying is controlled to be 100 to 130° C.; the vertical distance between the spray gun used for the plasma spraying and the rotary spray backing tube is 160 to 190 mm; (3) After the titanium dioxide target material is sprayed to a predetermined thickness, the plasma spraying is stopped and the rotary spraying backing tube is purged for 140 to 150 minutes, and the coolant temperature of the core shaft of the rotary spraying backing tube is set to be lowered to 20 to 30° C.; (4) After the titanium dioxide target material is cooled to room temperature, the preparation of the titanium dioxide target material is completed.
2. The method for preparing a titanium dioxide target according to claim 1, characterized in that: In the step (1), the outer diameter of the rotary spray backing tube is 120-150 mm, and the length is 300-500 mm.
3. The method for preparing a titanium dioxide target according to claim 1, characterized in that: In the step (2), the working current during the plasma spraying is 450-510A, the working voltage is 55-64V, the moving speed of the spray gun is 35-45mm / min, the rotation speed of the rotary spray back tube is 230-260rpm, the powder feeding amount is 92-96g / min, and the powder feeding gas flow rate is 2.4-2.9nL / min.
4. The method for preparing a titanium dioxide target according to claim 1, characterized in that: The spray gun is provided with a plasma generating pipeline, in which a mixed gas is provided. The mixed gas includes argon and hydrogen. The flow rate of the argon is 2200-2400 nL / h, and the flow rate of the hydrogen is 300-350 nL / h.
5. The method for preparing a titanium dioxide target according to claim 1, characterized in that: In the step (2), a dust removal device is also provided during the plasma spraying to perform dust removal, and the frequency of the dust removal device is 30 to 35 Hz.
6. The method for preparing a titanium dioxide target according to claim 1, characterized in that: In the step (2), the number of cooling air pipes is 2, and the air jets of the cooling air pipes are parallel to the spray gun muzzle of the plasma spraying machine and perpendicular to the axial direction of the rotary spraying back tube, and the vertical distance from the rotary spraying back tube is 20 to 30 mm.
7. The method for preparing a titanium dioxide target material according to claim 6, characterized in that: The interval between the two cooling air pipes is 100-200 mm, the inner diameter of the cooling air pipe is 6-8 mm, the outer diameter is 8-10 mm, the length is 150-200 mm, and the purge pressure is 3-4 kg.
8. The method for preparing a titanium dioxide target material according to claim 1, characterized in that: When the cooling air pipe is purging the titanium dioxide target in step (3), the rotation speed of the rotary spraying backing tube is 50 to 80 rpm.
9. The method for preparing a titanium dioxide target according to claim 1, characterized in that: The purity of the titanium dioxide powder is 99.95-99.99%, and the bulk density is 1.5-2 g / cm 3 .
10. The titanium dioxide target material prepared by the method for preparing a titanium dioxide target material according to any one of claims 1 to 8; preferably, the thickness of the titanium dioxide target material is ≥10 mm.