Preparation method and device of high-solid-content conductive paste
By grinding and stirring in the conductive paste preparation device, combining high-pressure air flow and mechanical stirring, carbon nanotubes and solvents are gradually increased, the problem of low solid content of carbon nanotubes in the conductive paste is solved, and dispersibility and conductivity are improved performance, reducing energy consumption and cost.
Patent Information
- Application Number
- CN202411211507.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The solid content of carbon nanotubes in existing conductive pastes is low, resulting in uneven dispersion, reducing conductive properties, and increasing energy consumption and production costs in subsequent electrode preparation.
Using a high solid content conductive paste preparation method, the carbon nanotubes are ground and mixed in the first mixing device of the conductive paste preparation device, and the second mixing device is used to stir and mix, and the solvent and Carbon nanotubes use high-pressure gas flow and mechanical stirring to promote dispersion, and finally dispersant is added to form a high solids conductive paste.
The dispersion and conductive properties of carbon nanotubes are improved, the concentration of carbon nanotubes in solvent is reduced, the difficulty of dispersion is reduced, and the formation of a high solid content conductive paste with stable performance is reduced, and production and transportation costs are reduced.
Smart Images

Figure CN119075790A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon nanotube production, and in particular to a method and a device for preparing a high-solid content conductive slurry. Background Art
[0002] Conductive paste is a material with conductive properties, and its main components include conductive materials, dispersants and matrix materials. Conductive materials are usually conductive particles, including metal particles, carbon nanotubes, graphene, etc.; dispersants are generally surfactants that can evenly disperse conductive particles to avoid aggregation and deposition of conductive particles; matrix materials are carriers of conductive particles, including organic polymers, ceramics, glass, etc. Conductive paste is widely used in the electronics industry, optoelectronics industry, medical industry, and aerospace industry due to its good conductive properties and conductive stability.
[0003] Carbon nanotubes are hollow tubular materials with a very high aspect ratio. Their unique tubular structure allows them to be inserted between matrix materials. After being mixed with the subsequent positive electrode materials and solidified, they form a strong conductive network, which significantly improves the conductive properties of the conductive paste. However, since carbon nanotubes have a very high specific surface area and strong van der Waals forces are formed between carbon nanotubes, different carbon nanotubes are very easy to agglomerate or entangle with each other, resulting in uneven dispersion of carbon nanotubes in the conductive paste, reducing the conductive properties of carbon nanotubes and subsequent electrode materials. The prior art usually reduces the solid content of carbon nanotubes in the conductive paste to ensure the dispersibility of carbon nanotubes in the conductive paste, but the low concentration of the conductive paste increases the energy consumption of the solvent evaporation and solvent purification process in the subsequent electrode preparation process, and there is also the problem of high production and transportation costs.
[0004] Existing conductive slurry preparation devices mainly include high-pressure homogenizers and sand mills, but the high-pressure homogenizer is mainly developed for layered graphite dispersion. Although the high-pressure homogenizer can disperse carbon nanotubes through pressure difference, it is generally a constant pressure during the working process. Therefore, it cannot be adjusted specifically according to the characteristics of the material to be dispersed. Summary of the invention
[0005] In view of the problem of low solid content in conductive paste in the prior art, the present invention provides a method and device for preparing a conductive paste with high solid content. First, the carbon nanotubes are ground and mixed for pretreatment by a first mixing device in the conductive paste preparation device to promote their agglomeration. Then, the pretreated paste is mixed with added solvent and carbon nanotubes respectively by alternately using a second mixing device and a first mixing device. This increases the solid content of the carbon nanotube conductive paste while ensuring good dispersion of the carbon nanotube conductive paste.
[0006] In a first aspect, the present invention provides a method for preparing a high solid content conductive paste, comprising the following steps: Step 1: adding carbon nanotubes and a solvent to a first mixing device according to a mass fraction of carbon nanotubes of not less than 20%, grinding and mixing, and obtaining a pre-treated slurry; Step 2: transferring the pretreated slurry obtained in step 1 to a second mixing device, and adding a solvent to the second mixing device for stirring and mixing; Step 3: Return the stirred and mixed slurry to the first mixing device, add carbon nanotubes to the first mixing device, and continue grinding and mixing; Step 4: Repeat steps 2-3 to obtain a dispersed slurry containing deagglomerated carbon nanotubes; Step 5: transferring the dispersed slurry containing the deagglomerated carbon nanotubes to a second mixing device, and adding a solvent equal to the amount of solvent added in step 2 to the second mixing device and mixing the mixture evenly to obtain a diluted slurry; Step 6: Add a dispersant to the diluted slurry obtained in step 5, and stir evenly to obtain a conductive slurry with a high solid content. The solvent is preferably at least one of N-methylpyrrolidone, N,N-dimethylformamide, ethanol, and water.
[0007] Furthermore, the carbon nanotubes are multi-walled carbon nanotubes with surface carboxylation.
[0008] Furthermore, in step 1, the mass fraction of carbon nanotubes is 20%-30%, such as 22%, 24%, 26%, 28% and so on.
[0009] Further, in step 2, the stirring and mixing includes mechanical stirring and mixing and high-pressure airflow stirring and mixing, the high-pressure airflow is a pulse airflow, the frequency of the pulse airflow is 70-100 times / hour, such as 75 times / hour, 80 times / hour, 85 times / hour, 90 times / hour, 95 times / hour, etc., each time lasts for 5-10 seconds, such as 6 seconds, 7 seconds, 8 seconds, 9 seconds, etc., and the pressure of the high-pressure airflow is 1-1.2 MPa. High-pressure gas is introduced into the second mixing device to form a high-pressure airflow to promote the pretreated slurry and the added solvent to be fully mixed in the second mixing device.
[0010] Furthermore, in step three, the mass of the carbon nanotubes added is less than 20% of the total mass of the solvent added in step two and the carbon nanotubes added in step three, preferably 10%-18%, such as 12%, 14%, 16%, etc.
[0011] Furthermore, the grinding speed is 2000-3000rpm, the grinding is preferably sand grinding, the sand grinding time is 0.5-2h, and the ball-to-material mass ratio of sand grinding is 8-10:1.
[0012] On the other hand, the present invention also provides a conductive paste preparation device used in the preparation method as described above, comprising a first mixing device, the first mixing device is connected to a second mixing device, the first mixing device is a sand mill, and the second mixing device is provided with a mechanical stirring device; The first mixing device is provided with a solid feed port and a first liquid feed port, the first liquid feed port is connected with the discharge port of the second mixing device, the discharge port of the first mixing device is connected with the feed port of the second mixing device, and the second mixing device is provided with a second liquid feed port.
[0013] Furthermore, the second mixing device is provided with a gas-liquid mixing device, the second mixing device is connected to a high-pressure gas source through the gas-liquid mixing device, the high-pressure gas source is connected to the pulse generator, and the high-pressure gas source is preferably a high-pressure nitrogen source or a high-pressure argon source. The mechanical stirring device and the pulse generator operate independently.
[0014] Furthermore, the gas inlet of the gas-liquid mixing device is connected to the high-pressure gas source, and the discharge port of the gas-liquid mixing device is connected to the second mixing equipment.
[0015] Furthermore, a conical guide tube is provided at the discharge port of the gas-liquid mixing device, the large-diameter end of the conical guide tube is connected to the discharge port of the gas-liquid mixing device, and the small-diameter end of the conical guide tube extends below the slurry liquid level inside the second mixing device. Such a design can increase the flow rate of the high-pressure airflow and increase the impact force of the high-pressure airflow on the slurry in the second mixing device. The high-pressure airflow from the high-pressure air source enters below the slurry liquid level inside the second mixing device through the conical guide tube, which can blow away the carbon nanotubes in the slurry inside the second mixing device, and the presence of the high-pressure airflow can further increase the vortex, promote the uniform mixing of the feed liquid, and improve the dispersion efficiency of the carbon nanotubes.
[0016] The beneficial effects of the present invention are: 1. The method for preparing a high-solid content conductive slurry provided by the present invention comprises the following steps: first, adding a portion of surface carboxylated carbon nanotubes and a portion of solvent to a first mixing device, and performing grinding and mixing pretreatment to form a pretreated slurry with a higher concentration of carbon nanotubes. The pretreated slurry is then transferred to a second mixing device, and a portion of solvent is added. After air flow stirring and mechanical stirring are performed to mix, the pretreated slurry is transferred to the first mixing device again to add a portion of carbon nanotubes for grinding to complete a cycle. The concentration of the carbon nanotubes added during one cycle is lower than the concentration of the carbon nanotubes in the slurry. This process is repeated multiple times. In order to gradually reduce the concentration of the carbon nanotubes in the slurry, a dispersant is added while adding the carbon nanotubes in the last cycle to prevent the obtained diluted slurry from agglomerating again. The slurry after adding the dispersant can be transported to the second mixing device, added with the solvent for mixing, and then discharged.
[0017] 2. The present invention improves the grinding efficiency of carbon nanotubes by preparing a pretreated slurry with a higher carbon nanotube concentration, and then gradually adds solvent and carbon nanotubes to the slurry to make the carbon nanotubes more easily dispersed. By controlling the amount of added solvent and carbon nanotubes, the concentration of carbon nanotubes in the solvent is gradually reduced, and finally a high-solid content conductive slurry with stable performance is formed.
[0018] 3. In the process of cyclically adding solvent and carbon nanotubes, the solvent is first added to the second mixing device to reduce the concentration of carbon nanotubes in the slurry accordingly, and then the carbon nanotubes are added to the first mixing device, which reduces the difficulty of dispersing the carbon nanotubes.
[0019] 4. The second mixing device is provided with both air flow stirring and mixing and mechanical stirring and mixing to promote further dispersion of the carbon nanotubes.
[0020] 5. The carbon nanotubes used in the present invention are carbonyl-treated carbon nanotubes, which are easier to disperse in subsequent treatments. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0022] Figure 1 Schematic diagram of the structure of the high-pressure sand mill dispersing device of Example 1.
[0023] In the figure, 1-sand mill, 11-solid feed port, 12-first liquid feed port, 121-first three-way valve, 122-first liquid discharge branch, 2-second mixing device, 3-second liquid feed port, 4-conical guide pipe, 411-gas-liquid mixing device, 5-filter membrane, 6-self-reflux pipeline, 611-second three-way valve, 612-third three-way valve, 7-second liquid discharge branch. DETAILED DESCRIPTION
[0024] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0025] Example 1 High-pressure sand mill dispersing device A high pressure sand mill dispersing device, such as Figure 1As shown, it includes a sand mill 1 and a second mixing device 2, the sand mill 1 is provided with a solid feed port 11 and a first liquid feed port 12, the first liquid feed port 12 is connected to a first three-way valve 121, the first three-way valve 121 is respectively connected to a solvent storage tank (not shown in the figure) and a first liquid discharge branch 122, the first liquid discharge branch 122 is connected to a second three-way valve 611, the second three-way valve 611 is respectively connected to a discharge port of the second mixing device 2 and a third three-way valve 612 through pipelines, and the other two interfaces of the third three-way valve 612 are respectively connected to a self-return pipeline 6 and a second liquid discharge branch. 7 is connected, a filter membrane 5 is arranged between the second three-way valve 611 and the third three-way valve 612, the free end of the second liquid discharge branch pipe 7 is connected to the second high-pressure gas source, the self-return pipeline 6 is connected to the liquid inlet of the gas-liquid mixing device 411, the gas inlet of the gas-liquid mixing device 411 is connected to the high-pressure nitrogen source through a pulse air pump, the discharge port of the gas-liquid mixing device 411 is connected to the large-diameter end of the tapered guide pipe 4, the small-diameter end of the tapered guide pipe 4 extends into the interior of the second mixing device 2 from the liquid return port of the second mixing device 2, and the gas-liquid mixing device 411 is a "T"-shaped hollow structure. The discharge port of the sand mill 1 is connected to the feed port of the second mixing device 2 through a pipeline, and a valve and a power pump are arranged on the pipeline between the discharge port of the sand mill 1 and the feed port of the second mixing device 2. The second mixing device 2 is provided with a second liquid feed port, and a mechanical stirring device is arranged inside the second mixing device 2, and the mechanical stirring device is preferably a mechanical stirring paddle. The mechanical stirring device and the pulse air pump operate independently. A cleaning liquid outlet is provided on the reflux pipeline 6 .
[0026] Instructions for use: The solvent and carbon nanotubes in the solvent storage tank enter the sand milling device through the first liquid feed port and the solid feed port respectively for sand milling treatment to obtain a pre-treated slurry with a mass fraction of carbon nanotubes not less than 20%. After the sand milling is completed, the valve and power pump set on the pipeline between the discharge port of the sand milling device and the feed port of the mixing device are opened to pump the pre-treated slurry in the sand milling device into the mixing device. At the same time, a certain amount of solvent is added to the mixing device from the second liquid feed port, and the pulse air pump and the mechanical stirring paddle inside the mixing device are turned on. The high-pressure nitrogen flow and mechanical stirring paddle output in the form of pulses are used to mechanically stir the liquid inside the mixing device and stir it with high-pressure air flow to promote secondary mixing of the pre-treated slurry and the newly added solvent. The frequency of the pulse is 70-100 times / hour, and each pulse lasts for 5-10s. The stirred liquid is discharged through the discharge port of the mixing device and the second liquid discharge branch of the reflux pipeline in turn. During the discharge of the liquid, the filter membrane can filter the liquid and intercept the solid particles in the liquid. After the liquid feed is discharged from the discharge port of the mixing device, the valve for controlling the pipeline between the second three-way valve and the first three-way valve is opened, and the stirred liquid feed can be passed into the sand mill again. At this time, carbon nanotubes are added to the sand mill, and the sand mill can be processed again to continue mixing the carbon nanotubes and the solvent in the sand mill, completing the first solvent addition, stirring, adding carbon nanotubes and grinding cycle. The ground liquid feed can be pumped into the mixing device again, and the second solvent addition, stirring, adding carbon nanotubes and grinding cycle is started. The solvent addition, stirring, adding carbon nanotubes and grinding cycle are repeated until the set number of cycles is completed to obtain a dispersed slurry of deagglomerated carbon nanotubes. The dispersed slurry of deagglomerated carbon nanotubes is pumped into the mixing device, and an equal amount of solvent as in the aforementioned cycle operation is added thereto, and a diluted slurry is obtained after stirring and mixing. A dispersant is added to the diluted slurry and stirred evenly to obtain a high solid content conductive slurry. The liquid feed filtered out by the filter membrane can also be passed into the mixing device through the reflux pipeline for stirring again. After the high-pressure sand mill dispersing device has been used for a period of time, the filter membrane will affect the discharge efficiency because some carbon nanotube particles remain on the side of the filter membrane facing the mixing device, and in severe cases, blockage may occur. In the high-pressure sand mill dispersing device provided by the present invention, the high-pressure airflow discharged from the second high-pressure air source can be introduced into the discharge side of the filter membrane through the third three-way valve. When cleaning the device, the filter membrane can be reversely purged through the third three-way valve by the high-pressure airflow, so that the residual carbon nanotubes remaining on the filter membrane are discharged from the high-pressure sand mill dispersing device from the cleaning liquid outlet along with the cleaning liquid, so as to complete the regeneration of the filter membrane.
[0027] Example 2 A high solid content conductive paste, the preparation method comprises the following steps: Step 1: Use the high-pressure sand milling dispersion device of Example 1 to pretreat the surface carboxylation multi-walled carbon nanotubes, and the pretreating process is as follows: 50.38 kg of N-methylpyrrolidone and 20.49 kg of surface carboxylation multi-walled carbon nanotubes are added to the sand mill through the first liquid feed port and the solid feed port, respectively, and sand milled in the sand mill to obtain a pretreated slurry. The sand milling speed is 3000 rpm, the sand milling time is 2 hours, and the sand milling medium is zirconia beads.
[0028] Step 2: The pretreated slurry after sand milling is discharged from the discharge port of the sand mill and enters the interior of the second mixing device. (10±0.5) kg of N-methylpyrrolidone is added to the second mixing device through the second liquid feed port. Mechanical stirring and high-pressure argon gas flow stirring are started at the same time. The mixture is stirred and mixed for 1 hour to obtain a mixed dispersed carbon nanotube slurry. N-methylpyrrolidone is added at one time. The high-pressure argon gas flow is pulsed into the slurry inside the second mixing device through the conical guide tube. The frequency of the pulse gas flow is 75 times / hour, each time lasting 6 seconds, and the pressure of the high-pressure nitrogen gas flow is 1 MPa.
[0029] Step 3: The mixed and dispersed carbon nanotube slurry is circulated into the sand mill through the discharge port of the second mixing device, the second three-way valve, the first liquid discharge branch pipe, the first three-way valve and the first liquid feed port in turn, and is sanded again. The sanding speed is 3000 rpm, the sanding time is 0.5 h, and the sanding medium is zirconia beads. At the same time, (2±0.3) kg of surface carboxylated multi-walled carbon nanotubes are added to the sand mill from the solid feed port and the sanding is continued for 1 h.
[0030] Step 4: Repeat steps 2 to 3 for five times to obtain a dispersed slurry of deagglomerated carbon nanotubes.
[0031] Step 5: Use a power pump to pump the dispersed slurry of the deagglomerated carbon nanotubes into the interior of the second mixing device through the pipeline set between the discharge port of the sand mill and the feed port of the second mixing device, and at the same time add (10±0.5) kg of N-methylpyrrolidone to the second mixing device through the second liquid feed port, and start mechanical stirring and high-pressure argon gas flow stirring at the same time, stir and mix for 1 hour to obtain a diluted slurry, and the diluted slurry is discharged from the high-pressure sand mill dispersion device through the filter membrane from the second liquid discharge branch. N-methylpyrrolidone is added once, and the high-pressure nitrogen gas flow is pulsed into the slurry inside the second mixing device through the conical guide pipe. The frequency of the pulse gas flow is 70 times / hour, each time lasting 10 seconds, and the pressure of the high-pressure nitrogen gas flow is 1MPa.
[0032] Step 6: Add 4.25 kg of dispersant hydrogenated nitrile rubber to the diluted slurry obtained in step 5, and stir evenly to obtain a high solid content conductive slurry, in which the mass fraction of carbon nanotubes is 20.13 wt%.
[0033] Example 3 A high solid content conductive paste, the preparation method comprises the following steps: Step 1: Use the high-pressure sand milling dispersion device of Example 1 to pretreat the surface carboxylation multi-walled carbon nanotubes, and the pretreating process is as follows: 80.76 kg of N-methylpyrrolidone and 20.45 kg of surface carboxylation multi-walled carbon nanotubes are added to the sand mill through the first liquid feed port and the solid feed port, respectively, and sand milled in the sand mill to obtain a pretreated slurry. The sand milling speed is 2500 rpm, the sand milling time is 3 hours, and the sand milling medium is zirconia beads.
[0034] Step 2: The pretreated slurry after sand milling is discharged from the discharge port of the sand mill and enters the interior of the second mixing device. (10±0.5) kg of N-methylpyrrolidone is added to the second mixing device through the second liquid feed port. Mechanical stirring and high-pressure argon gas flow stirring are started at the same time. The mixture is stirred and mixed for 1 hour to obtain a mixed dispersed carbon nanotube slurry. N-methylpyrrolidone is added at one time. The high-pressure argon gas flow is pulsed into the slurry inside the second mixing device through the conical guide tube. The pulse gas flow is emitted at a frequency of 80 times / hour, each time lasting 8 seconds. The pressure of the high-pressure nitrogen gas flow is 1.2 MPa.
[0035] Step 3: The mixed and dispersed carbon nanotube slurry is circulated into the sand mill through the discharge port of the second mixing device, the second three-way valve, the first liquid discharge branch pipe, the first three-way valve and the first liquid feed port in turn, and is sanded again. The sanding speed is 3000 rpm, the sanding time is 0.5 h, and the sanding medium is zirconia beads. At the same time, (2±0.3) kg of surface carboxylated multi-walled carbon nanotubes are added to the sand mill from the solid feed port and the sanding is continued for 1 h.
[0036] Step 4: Repeat steps 2 to 3 for five times to obtain a dispersed slurry of deagglomerated carbon nanotubes.
[0037] Step 5: Use a power pump to pump the dispersed slurry of the deagglomerated carbon nanotubes into the interior of the second mixing device through the pipeline set between the discharge port of the sand mill and the feed port of the second mixing device, and at the same time add (10±0.5) kg of N-methylpyrrolidone to the second mixing device through the second liquid feed port, and start mechanical stirring and high-pressure argon gas flow stirring at the same time, stir and mix for 1 hour to obtain a diluted slurry, and the diluted slurry is discharged from the high-pressure sand mill dispersion device through the filter membrane from the second liquid discharge branch. N-methylpyrrolidone is added once, and the high-pressure nitrogen gas flow is pulsed into the slurry inside the second mixing device through the conical guide pipe. The frequency of the pulse gas flow is 85 times / hour, each time lasting 8 seconds, and the pressure of the high-pressure nitrogen gas flow is 1.2MPa.
[0038] Step 6: Add 4.83 kg of dispersant hydrogenated nitrile rubber to the diluted slurry obtained in step 5, and stir evenly to obtain a high solid content conductive slurry, in which the mass fraction of carbon nanotubes is 17.35 wt%.
[0039] Example 4 A high solid content conductive paste, the preparation method comprises the following steps: Step 1: Use the high-pressure sand milling dispersion device of Example 1 to pretreat the surface carboxylation multi-walled carbon nanotubes, and the pretreating process is as follows: 150.36 kg of N-methylpyrrolidone and 40.58 kg of surface carboxylation multi-walled carbon nanotubes are added to the sand mill through the first liquid feed port and the solid feed port, respectively, and sand milled in the sand mill to obtain a pretreated slurry. The sand milling speed is 2000 rpm, the sand milling time is 2.5 hours, and the sand milling medium is zirconia beads.
[0040] Step 2: The pretreated slurry that has been sand-milled is discharged from the discharge port of the sand mill and enters the interior of the second mixing device. 15.49 kg of N-methylpyrrolidone is added to the second mixing device through the second liquid feed port. Mechanical stirring and high-pressure argon gas flow stirring are started at the same time. The mixture is stirred and mixed for 1 hour to obtain a mixed and dispersed carbon nanotube slurry. N-methylpyrrolidone is added at one time. The high-pressure argon gas flow is pulsed into the slurry inside the second mixing device through a conical feed pipe. The frequency of the pulsed gas flow is 80 times / hour, each time lasting 8 seconds, and the pressure of the high-pressure nitrogen gas flow is 1.2 MPa.
[0041] Step 3: The mixed and dispersed carbon nanotube slurry is circulated into the sand mill through the discharge port of the second mixing device, the second three-way valve, the first liquid discharge branch pipe, the first three-way valve and the first liquid feed port in turn, and is sanded again. The sanding speed is 3000 rpm, the sanding time is 0.5 h, and the sanding medium is zirconium oxide beads. At the same time, (2.5 ± 0.3) kg of surface carboxylated multi-walled carbon nanotubes are added to the sand mill from the solid feed port and the sanding is continued for 1 h.
[0042] Step 4: Repeat steps 2 to 3 for five times to obtain a dispersed slurry of deagglomerated carbon nanotubes.
[0043] Step 5: Use a power pump to pump the dispersed slurry of the deagglomerated carbon nanotubes into the interior of the second mixing device through the pipeline set between the discharge port of the sand mill and the feed port of the second mixing device, and at the same time add (15±0.5) kg of N-methylpyrrolidone to the second mixing device through the second liquid feed port, and start mechanical stirring and high-pressure argon gas flow stirring at the same time, stir and mix for 1 hour to obtain a diluted slurry, and the diluted slurry is discharged from the high-pressure sand mill dispersion device through the filter membrane from the second liquid discharge branch. N-methylpyrrolidone is added once, and the high-pressure nitrogen gas flow is pulsed into the slurry inside the second mixing device through the conical guide pipe. The frequency of the pulse gas flow is 85 times / hour, each time lasting 8 seconds, and the pressure of the high-pressure nitrogen gas flow is 1.2MPa.
[0044] Step 6: Add 6.37k dispersant hydrogenated nitrile rubber to the diluted slurry obtained in step 5, and stir evenly to obtain a high solid content conductive slurry, wherein the mass fraction of carbon nanotubes is 17.63wt%.
[0045] The electrode sheet resistivity test was carried out on the carbon nanotube conductive slurry prepared in Example 2-4. Lithium iron phosphate, carbon nanotube conductive slurry, polyvinylidene fluoride and N-methylpyrrolidone were homogenized in a mass ratio of 98:5:2:45, and then a 200 μm coating scraper was used to coat the homogenized slurry on the PI film, dried at 150°C for 1.5 h, and tested using a four-probe tester. The test data of the electrode sheet resistivity are shown in Table 1.
[0046] Table 1 Resistivity test results of carbon nanotube conductive pastes of Examples 2-4
[0047] As shown in Table 1, the mass fraction of carbon nanotubes in the high solid content conductive slurry obtained by the preparation process provided by the present invention is above 17%, and the electrode sheet resistivity is only 870-980Ω·m.
[0048] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and such modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily conceive of changes or substitutions within the technical scope disclosed by the present invention, and such changes or substitutions shall be within the scope of protection of the present invention.
Claims
1. A method for preparing a high solid content conductive paste, characterized in that: The steps include: Step 1: adding carbon nanotubes and a solvent to a first mixing device according to a mass fraction of carbon nanotubes of not less than 20%, grinding and mixing, and obtaining a pre-treated slurry; Step 2: transferring the pretreated slurry obtained in step 1 to a second mixing device, and adding a solvent to the second mixing device for stirring and mixing; Step 3: Return the stirred and mixed slurry to the first mixing device, add carbon nanotubes to the first mixing device, and continue grinding and mixing; Step 4: Repeat steps 2-3 to obtain a dispersed slurry containing deagglomerated carbon nanotubes; Step 5: transferring the dispersed slurry containing the deagglomerated carbon nanotubes to a second mixing device, and adding a solvent equal to the amount of solvent added in step 2 to the second mixing device and mixing the mixture evenly to obtain a diluted slurry; Step 6: Add a dispersant to the diluted slurry obtained in step 5, and stir evenly to obtain a conductive slurry with a high solid content.
2. The preparation method according to claim 1, characterized in that The carbon nanotubes are multi-walled carbon nanotubes with surface carboxyl groups.
3. The preparation method according to claim 1, characterized in that: In step 1, the mass fraction of carbon nanotubes is 20%-30%.
4. The preparation method according to claim 1, characterized in that: In step 2, the stirring and mixing includes mechanical stirring and mixing and high-pressure airflow stirring and mixing. The high-pressure airflow is a pulse airflow. The frequency of the pulse airflow is 70-100 times / hour, and each time lasts for 5-10 seconds.
5. The preparation method according to claim 1, characterized in that: In step three, the mass of the carbon nanotubes added is less than 20% of the total mass of the solvent added in step two and the carbon nanotubes added in step three.
6. The preparation method according to claim 1, characterized in that: The grinding speed is 2000-3000rpm.
7. A conductive paste preparation device used in the preparation method according to any one of claims 1 to 6, comprising a first mixing device, characterized in that: The first mixing device is connected to the second mixing device, the first mixing device is a sand mill, and the second mixing device is provided with a mechanical stirring device; The first mixing device is provided with a solid feed port and a first liquid feed port, the first liquid feed port is connected with the discharge port of the second mixing device, the discharge port of the first mixing device is connected with the feed port of the second mixing device, and the second mixing device is provided with a second liquid feed port.
8. The conductive paste preparation device according to claim 7, characterized in that: The second mixing device is provided with a gas-liquid mixing device, the second mixing device is connected with a high-pressure gas source through the gas-liquid mixing device, and the high-pressure gas source is connected with the pulse generator.
9. The conductive paste preparation device according to claim 8, characterized in that: The gas inlet of the gas-liquid mixing device is connected to the high-pressure gas source, and the discharge port of the gas-liquid mixing device is connected to the second mixing equipment.
10. The conductive paste preparation device according to claim 9, characterized in that: A conical guide pipe is arranged at the discharge port of the gas-liquid mixing device, the large-diameter end of the conical guide pipe is connected with the discharge port of the gas-liquid mixing device, and the small-diameter end of the conical guide pipe extends into the interior of the second mixing device.
Citation Information
Patent Citations
Carbon nanotube conductive slurry dispersing and mutual pouring system
CN111013471A
Device and method for preparing water-based carbon nanotube conductive paste
CN111346565A
Multi-point gas pulse mediating kettle
CN202860462U
Preparation device of oily carbon nanotube conductive paste with high solid content
CN216499001U
Sewage treatment agent mixing and dissolving device
CN217164156U
Cited By
Conductive slurry mixing and dispersing production cooperation automation control method
CN122230587A