Hole transport material with anion groups at two ends and battery

A hole transport material with anionic groups at both ends addresses charge recombination in perovskite solar cells by reducing electron concentration, thereby enhancing battery efficiency.

CN119080835APending Publication Date: 2024-12-06ZHEJIANG DASHENG NEW ENERGY TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411030099.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing perovskite solar cells suffer from charge recombination at the interface, limiting their efficiency below the theoretical limit, despite the use of self-assembled hole transport layers.

Method used

A hole transport material with anionic groups at both ends, synthesized from a specific structural substance, is anchored to ITO through phosphate groups, reducing electron concentration and inhibiting charge recombination.

Benefits of technology

The anionic groups repel electrons at the interface, lowering the electron-to-hole concentration ratio and enhancing battery performance by improving efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080835A_ABST
    Figure CN119080835A_ABST
Patent Text Reader

Abstract

The invention discloses a hole transport material with anion groups at two ends and a battery, the hole transport material at least comprises a material synthesized by a structural substance as shown in a formula I: # imgabs0 #, Y is one of carbazole, benzocarbazole or dibenzocarbazole, and # imgabs1 # is connected to a benzene ring; x is one of C, N, O, S and Se; r is one of # imgabs2 # and # imgabs3 #, and A and B are hydrogen ions or metal cations; the value range of n and m is 0-10, the hole transport material at least comprises a material synthesized from a structural substance shown in the formula I, the structural substance can be anchored with ITO through a phosphate group at the end part, and due to the fact that charges of the same polarity repel each other, anions in the group at the other end repel electrons at an interface, so that the concentration of the electrons at the interface can be reduced, and the hole transport efficiency is improved. The interface charge recombination is inhibited, and the performance of the battery, such as the battery efficiency, is favorably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of batteries, and in particular to a hole transport material with anion groups at both ends and a battery. Background Art

[0002] Perovskite solar cells (PSCs) are a promising new photovoltaic technology with high conversion efficiency and low cost. Perovskite solar cells contain a hole transport layer, a perovskite light absorption layer and an electron transport layer. The holes and electrons in the perovskite light absorption layer enter the hole transport layer and the electron transport layer respectively, and then reach the electrode to generate photocurrent. The hole transport layer and the electron transport layer are crucial to the performance and stability of the device.

[0003] At present, in order to improve efficiency, some researchers use chemical anchoring on transparent conductive oxide electrodes to synthesize hole transport materials using self-assembled molecules (SAM). This type of self-assembled hole transport layer is conducive to achieving high efficiency of photovoltaic devices, but it is still lower than its theoretical limit efficiency. One of the reasons is the charge recombination at the interface, which requires further research and development and improvement. Summary of the invention

[0004] To solve at least one of the above technical defects, the present invention provides the following technical solutions:

[0005] The first aspect of the present application document discloses a hole transport material with anionic groups at both ends, comprising at least a material synthesized from a structural substance as shown in Formula 1,

[0006] Formula 1:

[0007] wherein Y is one of carbazole, benzocarbazole or dibenzocarbazole, and Attached to the benzene ring;

[0008] X is one of C, N, O, S and Se;

[0009] R is One of the following, wherein A and B are hydrogen ions or metal cations;

[0010] The value range of n and m is 0-10.

[0011] Furthermore, A and B are one of hydrogen ion, potassium ion, sodium ion, lithium ion, cesium ion, rubidium ion, beryllium ion, magnesium ion, calcium ion, strontium ion and barium ion.

[0012] Further, a mixed solution of the structural material shown in Formula 1 and a solvent is coated and treated at 60-120° C. for 5-25 min to obtain a hole transport material.

[0013] further, At least two benzene rings connected to both sides of nitrogen, (X) n The number of C double bonds in the molecule is ≥ 0.

[0014] Further, the substance of formula 1 is any one of the following:

[0015]

[0016]

[0017] The second aspect of the present application discloses a battery comprising any of the hole transport materials described above.

[0018] Furthermore, the battery is a single-cell perovskite type or a perovskite / heterojunction stacked type.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The hole transport material of the present invention at least includes a material synthesized by the structural substance shown in Formula 1. The structural substance can be anchored to ITO through the phosphate group at the end, and because like charges repel each other, the anion in the other end group repels electrons at the interface, thereby reducing the concentration of electrons at the interface, reducing the concentration ratio between electrons and holes, inhibiting the interface charge recombination rate, and helping to improve the performance of the battery, such as battery efficiency. DETAILED DESCRIPTION

[0021] The present invention will be further described below in conjunction with specific embodiments.

[0022] For the Y group, Among them, when the value of n is 0, the R group is directly connected to the benzene ring.

[0023] For the preparation of the substance of formula 1, if it is purchased directly from the market or synthesized by oneself, the following synthetic routes can be selected:

[0024]

[0025]

[0026] 1 equivalent of carbazole 9a and an appropriate amount of DMF were placed in a three-necked flask, placed in an ice-water bath, and stirred for one hour in a nitrogen atmosphere. After that, 2 equivalents of N-bromosuccinimide DMF solution were added dropwise. The mixture was reacted at room temperature for 10 hours. An appropriate amount of deionized water was added to precipitate, which was filtered, washed, dried, and recrystallized from dichloromethane to obtain compound 9b.

[0027] 1 equivalent of 9b was dissolved in an appropriate amount of ether, and 1.07 equivalents of n-butyl lithium hexane solution was added dropwise at 0 degrees. After the addition, stirring was continued for one hour. 1.06 equivalents of trimethylsilyl chloride was added at room temperature. After stirring at room temperature for one hour, the reaction mixture was cooled to -78°C, and four equivalents of tert-butyl lithium pentane solution were added. The suspension was continued to be stirred at 0°C for 3 hours, and 5 equivalents of iodomethane were added. The reaction mixture was reacted overnight at room temperature. The reaction mixture was hydrogenated with an appropriate amount of 1M HCl, the two phases were separated, and the organic layer was washed with 1M HCl and pure water, dried over anhydrous magnesium sulfate, and recrystallized to obtain compound 9c.

[0028] One equivalent of 9c was dissolved in excess 1,2-dibromoethane, 0.25 equivalent of tetra-n-butylammonium bromide and 10 equivalents of 50% KOH solution. The mixture was heated to 70°C and stirred overnight. After the reaction was completed, it was extracted with DCM, and the organic layer was dried over anhydrous sodium sulfate and concentrated to obtain compound 9d.

[0029] 1 equivalent of 9d was dissolved in 35 equivalents of triethyl phosphite, and the reaction mixture was heated to 140°C overnight. The solvent was removed in vacuo, and after column chromatography purification, the intermediate product was dissolved in an appropriate amount of anhydrous 1,4-dioxane in a nitrogen atmosphere, and trimethylsilyl bromide was added dropwise to the mixed solution. The reaction mixture was reacted at room temperature overnight, and after adding an appropriate amount of methanol, stirring was continued for three hours. Finally, deionized water was added dropwise until the solution became turbid, and stirring was continued for two hours. After the reaction was completed, it was filtered, washed with water, and recrystallized to obtain compound 9e.

[0030] 1 equivalent of 9e and 30 equivalents of triethyl orthoacetate were stirred at 90°C for 24 hours. After the reaction was completed, the orthoester was removed in vacuo and purified by column chromatography to obtain compound 9f.

[0031] At room temperature, add 1.1 equivalents of 1,3-dibromo-5,5-dimethylhydantoin (DBH) and 0.1 equivalents of azoisobutyronitrile (AIBN) to 1 equivalent of 9f acetonitrile solution, heat and stir to 90°C, and react for two hours. Cool, filter, discard insoluble matter, evaporate the solvent from the filtrate under reduced pressure, and chromatograph the residue on a silica gel column to obtain compound 9g.

[0032] Add appropriate amount of ethanol and water to the flask, then add sodium disulfide, stir for 1.5h, slowly drop 9g ethanol solution, react at reflux temperature after adding, control the reaction temperature to 70℃, and stir for 8h. Extract with dichloromethane, separate the phases, concentrate the organic phase to obtain disulfide. Then add disulfide to the flask, add reducing agent Fe / HCl, add iron, slowly drop 20% HCl, maintain the temperature at 20℃, stir for 10h, and the reaction is over. Compound 9h is obtained.

[0033] To the solution of compound 9h and potassium hydroxide, add a calculated amount of hydrogen peroxide solution dropwise under magnetic stirring in an ice bath, then stir at room temperature for four to five hours to stop the reaction, adjust the pH value to neutral with glacial acetic acid, then evaporate part of the solvent, adjust the pH value to about 3-4, put it in a refrigerator, and freeze it at about 5 degrees for 12 hours. After crystals precipitate, filter it to obtain compound 9i.

[0034] Under nitrogen protection, 2 equivalents of triethylamine and then 6 equivalents of trimethylsilyl bromide were added to 1 equivalent of 9i in chloroform solution. The reaction was allowed to proceed overnight. The solution was concentrated, washed with an appropriate amount of organic solvent, and the solvent was removed in vacuo to obtain compound 9j.

[0035] Prepare 4 equivalents of KOH in a 15 wt% aqueous solution, slowly add 9j dropwise at room temperature, and after the acid is added, adjust the pH to 8 to obtain compound 9.

[0036]

[0037] Phosphorus oxychloride was added to anhydrous DMF at 0°C, stirred at low temperature for half an hour, 2a dissolved in dichloromethane was added, and stirring continued until room temperature, and finally heated to 80°C, reacted for 2 hours, and finally quenched with an ice-water bath, adjusted pH, extracted, washed with brine, and dried to obtain compound 2b.

[0038] At 10 degrees Celsius, 2b, KH 2 PO 4 , hydrogen peroxide, and polyethylene glycol are suspended in a mixture of ACN and water, and an aqueous solution of sodium chlorite is added dropwise within two hours. After the addition is completed, the mixture is stirred at room temperature overnight. Sodium sulfite is added to the system, and the pH value of the system is adjusted to 3 with 10% hydrochloric acid. The mixture is extracted with ether, and the organic phase is washed once with a sodium bisulfite solution and once with water, dried, filtered, and concentrated to obtain the intermediate product 2c.

[0039] The synthesis of the last two steps of compounds 2 and 1 is shown in the synthesis of compounds 9j and 9.

[0040]

[0041] Under nitrogen protection, 2b was dissolved in anhydrous ethanol and tetrahydrofuran, and NaBH 4 , stirred at room temperature overnight. After the reaction was completed, the mixed solution was poured into water to quench the reaction, extracted with chloroform and dried over magnesium sulfate. The crude product was separated by column chromatography to obtain intermediate 3a.

[0042] Add intermediate 3a to triethyl phosphate, cool in an ice-water bath, then add iodine to the mixed solution and stir overnight at room temperature. After the reaction is completed, remove the remaining triethyl phosphate by vacuum distillation. Wash the crude product with water and extract with chloroform. The crude product is separated by column chromatography to obtain intermediate 3b.

[0043] The crude product was dissolved in a mixed solvent of ethanol / tetrahydrofuran / water, potassium hydroxide was added to the mixed solution, and the mixture was refluxed for 1 hour. After the reaction was completed, the solvent was removed by rotary evaporation. Hydrochloric acid was added to adjust the pH to 5. The precipitated precipitate was purified by recrystallization with ethanol to obtain product 3.

[0044] The synthesis of compound 4 in the last step reaction is shown in the last step of the synthesis procedure of 9.

[0045]

[0046] 1 equivalent of 9b was dissolved in excess 1,2-dibromoethane, 0.25 equivalent of tetra-n-butylammonium bromide and 10 equivalents of 50% KOH solution. The mixture was heated to 70°C and stirred overnight. After the reaction was completed, it was extracted with DCM, and the organic layer was dried over anhydrous sodium sulfate and concentrated to obtain 5a.

[0047] One equivalent of 5a was dissolved in 40 equivalents of triethyl phosphite, and the reaction mixture was heated to 140°C overnight. The solvent was removed in vacuo, and after column chromatography purification, the intermediate product was dissolved in an appropriate amount of anhydrous 1,4-dioxane in a nitrogen atmosphere, and trimethylsilyl bromide was added dropwise to the mixed solution. The reaction mixture was reacted at room temperature overnight, and after adding an appropriate amount of methanol, stirring was continued for three hours. Finally, deionized water was added dropwise until the solution became turbid, and stirring was continued for two hours. After the reaction was completed, it was filtered, washed with water, and recrystallized to obtain the intermediate product 5b.

[0048] The synthesis of the last step reaction compound 5 can be seen in the last two steps of the synthesis procedure of compound 9.

[0049]

[0050] Under nitrogen atmosphere, add 9 g of tetramethyl methylene diphosphonate, 1,8-diazobispiro[5.4.0]undec-7-ene (DBU), and tetrahydrofuran into a round-bottom flask. React at room temperature for two hours. After the reaction is completed, dilute with water and add an appropriate amount of ethyl acetate to dissolve. Wash the organic phase with water several times, dry with anhydrous sodium sulfate, and concentrate to obtain compound 6a.

[0051] The synthesis of the last step compound 6 is shown in the synthesis of compounds 9j and 9.

[0052]

[0053] Under nitrogen atmosphere, 2b, tetramethylmethylene diphosphonate, toluene, and piperidine were added to a round-bottom flask. The mixture was heated to 110°C and reacted for ten hours. After the reaction was completed, the organic solvent was removed in vacuo, and the solid was dissolved with dichloromethane, dried over anhydrous sodium sulfate, and the solvent was removed in vacuo. The product 7a was obtained by column chromatography.

[0054] The synthesis of the last step compound 7 is shown in the synthesis of compounds 9j and 9.

[0055] The synthesis method of the structural formula in Example 8 below is similar to that of Example 7, except that in the first step, tetramethylmethylene diphosphonate is replaced with ethyl cyanoacetate.

[0056] The battery is prepared as follows:

[0057] For example, a single perovskite battery uses a two-step method:

[0058] (1) laser cutting to obtain FTO conductive glass with a specification of 6×6 cm for later use;

[0059] (2) Preparation of nickel oxide layer:

[0060] A nickel oxide ethanol dispersion with a concentration of 20 g / mL was prepared, and the dispersion was spin-coated on the conductive surface of the FTO conductive glass at a rotation speed of 2000 rpm for 30 seconds, and annealed at 100° C. for 10 minutes to obtain a laminated structure of FTO / nickel oxide layer;

[0061] (3) Preparation of a hole transport material with anionic groups at both ends:

[0062] An isopropanol dispersion with a concentration of 1 g / mL was prepared, and the surface of the nickel oxide layer away from the FTO conductive glass was spin-coated at a speed of 3000 rpm for 30 seconds, and annealed at 100°C for 10 minutes to obtain a stacked structure of FTO / nickel oxide layer / terminal anion hole transport layer;

[0063] (4) Preparation of lead salt film:

[0064] The stacked structure of FTO / nickel oxide layer / terminal anion hole transport layer with a specification of 6×6 cm prepared in step (3) is transferred to a vacuum evaporation device 500, and lead iodide and cesium iodide are used as evaporation sources to form a lead salt film on the surface of Example 1 at 1×10-5 Pa and 450° C. to obtain a stacked structure of FTO / nickel oxide layer / terminal anion hole transport layer / Cs0.05Pb2.05 layer, which is used as a base film layer A for standby use;

[0065] (5) Preparation of perovskite active layer:

[0066] An isopropanol dispersion of a mixture of FAI and MACl was prepared, wherein the concentration of FAI was 80 mg / mL and the concentration of MACl was 6 mg / mL, and the dispersion was dropped onto the above substrate. The dispersion was spin-coated at 3000 rpm for 30 seconds and then annealed at 150°C for 15 minutes to obtain a perovskite film.

[0067] (6) PEAI, C60, BCP and Ag are sequentially deposited on FTO / nickel oxide layer / example 1 / perovskite layer to obtain a perovskite cell, whose structure is FTO / nickel oxide layer / terminal anion hole transport layer / perovskite layer / PEAI / C60 / BCP / Ag.

[0068] Such as perovskite / heterojunction stacked cells

[0069] 1. N type <100> A polished Cz silicon wafer substrate with a crystal orientation is placed in a PECVD system, and a layer of intrinsic hydrogenated amorphous silicon is deposited on the front and back sides of the silicon wafer to obtain a first intrinsic hydrogenated non-silicon layer / n-type crystalline silicon layer / second intrinsic hydrogenated silicon layer amorphous silicon wafer.

[0070] 2. Depositing p-type doped amorphous silicon on the first intrinsic hydrogenated amorphous silicon to form a p-type doped amorphous silicon layer, to obtain a p-type doped amorphous silicon layer / first intrinsic hydrogenated amorphous silicon layer / n-type crystalline silicon layer / second intrinsic hydrogenated silicon layer amorphous silicon wafer.

[0071] 3. Depositing n-type doped nano-silicon oxide on the second intrinsic hydrogenated amorphous silicon to form an n-type doped nano-silicon oxide layer, thereby obtaining a p-type doped amorphous silicon layer / first intrinsic hydrogenated non-silicon layer / n-type crystalline silicon layer / second intrinsic hydrogenated amorphous silicon layer / n-type doped nano-silicon oxide silicon sheet layer.

[0072] 4. Using magnetron sputtering deposition technology, at a power of 70 W, a layer of indium tin oxide was deposited on the p-type doped amorphous silicon layer and the n-type doped nano silicon oxide layer, respectively, to form a first indium tin oxide layer and a second indium tin oxide layer, and a first indium tin oxide layer / p-type doped amorphous silicon layer / first intrinsic hydrogenated non-silicon layer / n-type crystalline silicon layer / second intrinsic hydrogenated amorphous silicon layer / n-type doped nano silicon oxide layer / second indium tin oxide layer stacked structure was obtained.

[0073] 5. On the indium tin oxide layer close to the n-type crystalline silicon layer, an isopropyl alcohol dispersion of terminal anion groups is spin-coated at a rotation speed of 3000 rpm / s, and then annealed at 100°C for 10 minutes to form a terminal anion hole transport layer, thereby obtaining a stacked structure of first indium tin oxide layer / p-type doped amorphous silicon layer / first intrinsic hydrogenated non-silicon layer / n-type crystalline silicon layer / second intrinsic hydrogenated amorphous silicon layer / n-type doped nano-silicon oxide layer / second indium tin oxide layer / terminal anion hole transport layer; wherein the concentration of the isopropyl alcohol dispersion is 1 mg / mL.

[0074] 6. Under the conditions of 1×10-6Pa and 450°C, lead iodide, lead bromide and cesium iodide are evaporated and deposited on the terminal anion hole transport layer to form a Cs0.2PbI1.5Br0.7 layer to obtain a first indium tin oxide layer / p-type doped amorphous silicon layer / first intrinsic hydrogenated non-silicon layer / n-type crystalline silicon layer / second intrinsic hydrogenated amorphous silicon layer / n-type doped nano-silicon oxide layer / second indium tin oxide layer / terminal anion hole transport layer / Cs0.2PbI1.5Br0.7 layer stacked structure.

[0075] 7. Prepare a 50 g / mL dispersion of formamidine iodide (FAI) and 5 mg / mL (methylamine chloride) MACl in isopropanol, spin coat it on the Cs0.2PbI1.5Br0.7 layer at 3000 rpm for 30 seconds, and anneal at 150°C for 10 minutes.

[0076] 8. Prepare a PEAI isopropanol dispersion with a concentration of 1 g / mL, deposit PEAI on the FA0.8Cs0.2PbI2.3Br0.7 layer at a rotation speed of 3000 rpm to form a PEAI layer, spin coat for 30 seconds, and anneal at 100°C for 10 minutes to obtain a first indium tin oxide layer / p-type doped amorphous silicon layer / first intrinsic hydrogenated non-silicon layer / n-type crystalline silicon layer / second intrinsic hydrogenated amorphous silicon layer / n-type doped nano-silicon oxide layer / second indium tin oxide layer / terminal anion hole transport layer / Cs0.2PbI 1.5Br0.7 layer / PEAI layer stacked structure.

[0077] 9. Under the conditions of 1×10-6Pa and 250°C, a 20nm carbon 60 layer was evaporated and deposited on the PEAI layer, and then a 20nm tin dioxide layer was deposited on the carbon 60 layer by atomic layer deposition technology to obtain a first indium tin oxide layer / p-type doped amorphous silicon layer / first intrinsic hydrogenated non-silicon layer / n-type crystalline silicon layer / second intrinsic hydrogenated amorphous silicon layer / n-type doped nano-silicon oxide layer / second indium tin oxide layer / terminal anion hole transport layer / Cs0.2PbI1.5Br0.7 layer / PEAI layer / carbon 60 layer / tin dioxide layer stacked structure.

[0078] 10. Indium tin oxide is deposited on the tin dioxide layer by magnetron sputtering to form a third indium tin oxide layer, to obtain a stacked structure of first indium tin oxide layer / p-type doped amorphous silicon layer / first intrinsic hydrogenated non-silicon layer / n-type crystalline silicon layer / second intrinsic hydrogenated amorphous silicon layer / n-type doped nano-silicon oxide layer / second indium tin oxide layer / terminal anion hole transport layer / Cs0.2PbI1.5Br0.7 layer / PEAI layer / carbon 60 layer / tin dioxide layer / third indium tin oxide layer.

[0079] 11. The front and back surfaces of the stacked structure obtained in step (11) are respectively screen-printed with silver paste to form a first metal silver layer and a second metal silver layer, and sintered at 200° C. to obtain a perovskite / crystalline silicon stacked battery (first metal silver layer / first indium tin oxide layer / p-type doped amorphous silicon layer / first intrinsic hydrogenated non-silicon layer / n-type crystalline silicon layer / second intrinsic hydrogenated amorphous silicon layer / n-type doped nano-silicon oxide layer / second indium tin oxide layer / terminal anion hole transport layer / Cs0.2PbI1.5Br0.7 layer / PEAI layer / carbon 60 layer / tin dioxide layer / third indium tin oxide layer / second metal silver layer).

[0080] Example 1

[0081] The perovskite / heterojunction stacked cell is prepared by the above method, wherein the structural formula 1 is:

[0082]

[0083] Example 2

[0084] The difference from Example 1 is that the structural formula of Formula 1 is:

[0085]

[0086] Example 3

[0087] The difference from Example 1 is that the structural formula of Formula 1 is:

[0088] Example 4

[0089] The difference from Example 1 is that the structural formula of Formula 1 is:

[0090] Example 5

[0091] The difference from Example 1 is: Structural formula:

[0092]

[0093] Example 6

[0094] The difference from Example 1 is that the structural formula of Formula 1 is:

[0095]

[0096] Example 7

[0097] The difference from Example 1 is that the structural formula of Formula 1 is:

[0098]

[0099] Example 8

[0100] The difference from Example 1 is that the structural formula of Formula 1 is:

[0101]

[0102] Example 9

[0103] The difference from Example 1 is that the structural formula of Formula 1 is:

[0104]

[0105] Comparative Example 1

[0106] Compared with Example 1, the difference is that the hole transport layer is

[0107]

[0108] Comparative Example 2

[0109] Compared with Example 1, the difference is that the hole transport layer is

[0110]

[0111] Comparative Example 3

[0112] Compared with Example 1, the difference is that the hole transport layer is

[0113]

[0114] The performance of the batteries prepared above was tested, as shown in Table 1. It can be seen that the batteries in Examples 1-13 have improved battery efficiency and other performances. This shows that the scheme of adjusting the electronic interface composite with anionic groups is completely feasible and worthy of further development and promotion.

[0115] Table 1: Effects of different self-assembly materials on the performance of stacked batteries

[0116]

[0117]

[0118] The above are only preferred embodiments of the present invention. The protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A hole transport material with anionic groups at both ends, It is characterized in that A material comprising at least one structural substance as shown in Formula 1, Formula 1: wherein Y is one of carbazole, benzocarbazole or dibenzocarbazole, and Attached to the benzene ring; X is one of C, N, O, S and Se; R is One of the following, wherein A and B are hydrogen ions or metal cations; The value range of n and m is 0-10.

2. A hole transport material with anionic groups at both ends as claimed in claim 1, Features: A and B are one of hydrogen ion, potassium ion, sodium ion, lithium ion, cesium ion, rubidium ion, beryllium ion, magnesium ion, calcium ion, strontium ion and barium ion.

3. A hole transport material with anionic groups at both ends as claimed in claim 1, Features: A mixed solution of the structural material shown in Formula 1 and a solvent is coated and treated at 60-120° C. for 5-25 minutes to obtain a hole transport material.

4. A hole transport material with anionic groups at both ends as claimed in claim 1, Features: At least two benzene rings connected to both sides of nitrogen, (X) n The number of C double bonds in the molecule is ≥ 0.

5. A hole transport material with anionic groups at both ends as claimed in claim 4, Features: The substance of formula 1 is any of the following: 6.Battery, Features: The method comprises the hole transport material according to any one of claims 1 to 5.

7. The battery according to claim 6, Features: The battery is of a single-cell perovskite type or a perovskite / heterojunction stacked type.

Citation Information

Patent Citations

  • Organic hole transport material and perovskite solar cell prepared from same

    CN115322121A

  • Hole transport material containing benzene ring and heterocyclic ring structure and application of hole transport material

    CN117603266A

  • Functional material, passive film, solar cell, photovoltaic module and photovoltaic system