A kind of dyeing method of nylon
A nylon and fabric dyeing technology, which is applied in the field of nylon dyeing, can solve the problems of high chemical composition measurement requirements, complex realization, and ineffective improvement of color fastness, and achieve process stability, process control, and high color fastness to washing. Effect
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2019-08-27
Smart Images

Figure 1
Abstract
Description
Technical field
[0001] The invention belongs to the technical field of textile dyeing, and specifically relates to a dyeing method of nylon. Background technique
[0002] Fibers are divided into chemical fibers and natural fibers. Among them, chemical fibers are fibers with textile properties that are made from natural polymer compounds or synthetic polymer compounds as raw materials, through the preparation of spinning dope, spinning, and post-processing. It has the advantages of light resistance, abrasion resistance, easy to wash and dry, no mildew, no insects, etc. It is widely used in the manufacture of clothing fabrics, filter cloths, conveyor belts, hoses, ropes, fishing nets, electrical insulation wires, medical sutures, tire cord fabrics and parachutes, etc.
[0003] Nylon (commonly known as nylon), whose scientific name is polyamide fiber, is one of the chemical fibers and is the first synthetic fiber in the world. Compared with polyester and acrylic, nylon has the advan...
Examples
Embodiment 1
[0028] ① Immerse 500kg of cotton fabric in the first dyeing solution containing 1.0gHT-33N and 0.05g SunacidOrange GSN per liter (the total weight of the acid dye is 0.05% of the fabric weight), add 1M hydrochloric acid to adjust the pH to 4.0, Then treat at 98°C for 40 minutes, and then cool to below 60°C to drain;
[0029] ②The fabric treated in step ① is soaped at 40℃ for 20 minutes and then drained;
[0030] ③The fabric treated in step ② is washed at room temperature first, and after draining, it is acid-fixed at 60°C for 30 minutes;
[0031] ④The fabric treated in step ③ is immersed in 35°C hot water containing high molecular polymer and washed for 25 minutes. After draining, it is washed at room temperature.
Embodiment 2
[0033] ①Soak 500kg of cotton fabric in the first dyeing solution containing 2.0g HT-33N and 3.0g Sunacid Orange GSN per liter (the total weight of the acid dye is 0.5% of the fabric weight), and add 2M hydrochloric acid to adjust the pH to 4.5 , Then treat it at 98℃ for 30min, then cool to below 60℃ to drain;
[0034] ②The fabric treated in step ① is soaped at 40°C for 15 minutes and drained;
[0035] ③The fabric treated in step ② is washed at room temperature first, and after draining, it is acid-fixed at 65°C for 15 minutes;
[0036] ④The fabric treated in step ③ is immersed in 35°C hot water containing special high molecular polymers and washed for 25 minutes. After draining, it is washed at room temperature.
Embodiment 3
[0038] ① Immerse 500kg of cotton fabric in the first dye liquor containing 1.8g HT-33N and 2.05g SunacidOrange GSN per liter (the total weight of the acid dye is 1.5% of the fabric weight), and add 1.5M hydrochloric acid to adjust the pH 4.8, then treat at 100℃ for 30min, and then cool to below 60℃ to drain;
[0039] ②The fabric treated in step ① is soaped at 50°C for 18 minutes and drained;
[0040] ③The fabric treated in step ② is washed at room temperature first, and after draining, it is acid-fixed at 75°C for 20 minutes;
[0041] ④The fabric treated in step ③ is immersed in hot water containing a special polymer at 42°C and washed for 18 minutes. After draining, it is washed at room temperature.