Preparation method of Al-doped ZnO low-resistivity nano powder

By using cationic magnetic microspheres and magnetic separation method under acidic conditions in Al-doped ZnO powder, anions are removed, and the problems of powder agglomeration and high resistivity are solved, and the preparation of nano powder with high stability and low resistivity is achieved. , suitable for industrial production.

CN118908266APending Publication Date: 2024-11-08CHANGDI NEW MATERIAL TECHNOLOGY (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410952488.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Al-doped ZnO powder is easily agglomerated due to its high surface energy and anion adsorption, which is difficult to remove during the calcination process, resulting in high resistivity and affecting its application.

Method used

The cationic magnetic microspheres are mixed with the precipitate under acidic conditions, and the cationic magnetic microspheres are removed by magnetic separation, which reduces the anion content, improves the dimensional stability of the nano powder, and enhances the preparation method of cationic magnetic microspheres. Adsorption and removal of anions.

Benefits of technology

It effectively improves the dimensional stability and purity of Al-doped ZnO low-resistivity nano powder, reduces the resistivity, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908266A_ABST
    Figure CN118908266A_ABST
Patent Text Reader

Abstract

The invention relates to the field of low-resistivity photoelectric nano powder materials, and particularly discloses a preparation method of Al-doped ZnO low-resistivity nano powder. A preparation method of Al-doped ZnO low-resistivity nano powder comprises the following preparation steps: stirring and mixing aluminum salt, zinc salt and water, adding an aqueous solution of alkali, and stirring and mixing to obtain a sol solution; centrifuging the sol solution to obtain a precipitate; mixing the precipitate, cationic magnetic microspheres and water, adjusting the pH value to 2-5, stirring and mixing, removing the cationic magnetic microspheres by adopting a magnetic separation method, filtering, washing and drying to obtain a dried precipitate; and crushing and calcining the dried precipitate, so as to obtain the Al-doped ZnO low-resistivity nano powder. The cation magnetic microspheres can effectively remove anions in the precipitate, so that the calcined precipitate is not easy to sinter, and the size stability of the Al-doped ZnO low-resistivity nano powder is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of low-resistivity optoelectronic nanopowder materials, and more specifically, to a method for preparing Al-doped ZnO low-resistivity nanopowder. Background Art

[0002] Among the third generation n-type semiconductors of the II-VI group, ZnO has received extensive attention due to its unique optoelectronic properties. As a typical wide bandgap (3.37 eV at room temperature) semiconductor material, ZnO has a series of excellent optoelectronic properties including optoelectronics, piezoelectricity, gas sensing and pressure sensing, and has a high exciton binding energy (60 meV). Therefore, it has been widely used in the fields of light-emitting elements, optical waveguides, transparent semiconductor conductive materials, high-frequency piezoelectric transducers, low-voltage varistors and microsensors.

[0003] Doping is an effective method to improve the performance of nanomaterials. After ZnO is doped with Al, its photoelectric performance is further optimized compared with ZnO, which is comparable to the classic ITO. In addition, Zn and Al are abundant, non-toxic, cheap, and have a variety of preparation technologies.

[0004] At present, chemical precipitation is one of the commonly used methods for preparing Al-doped ZnO powder because of its simple process, convenient operation, low requirements on equipment, and easy industrial production. The chemical precipitation method mainly uses soluble salts of zinc and aluminum and urea to heat in water, and urea decomposes ammonia water to react with soluble salts of zinc and aluminum to form a precursor precipitate. The precursor precipitate is washed and filtered several times to remove impurities such as anions in the precipitate, and then calcined to produce Al-doped ZnO powder.

[0005] Because Al-doped ZnO powder has a large specific surface area and high surface energy, anions are easily adsorbed on the surface of Al-doped ZnO powder and are difficult to remove by washing. However, the anions contained between the precipitates will produce salt bridges and sintering during the calcination process, making Al-doped ZnO powder easy to agglomerate. Summary of the invention

[0006] In order to improve the dimensional stability of Al-doped ZnO powder and reduce powder agglomeration, the present application provides a method for preparing Al-doped ZnO low-resistivity nanopowder.

[0007] In a first aspect, the present application provides a method for preparing Al-doped ZnO low resistivity nanopowder, using the following technical solution: A method for preparing Al-doped ZnO low-resistivity nanopowder comprises the following preparation steps: S1: stirring and mixing aluminum salt, zinc salt and water to obtain a reaction precursor solution; S2: adding the aqueous solution of alkali dropwise into the reaction precursor solution, stirring and mixing, to obtain a sol solution; S3: centrifuging the sol solution to obtain a precipitate; S4: after mixing the precipitate, cationic magnetic microspheres and water, adjusting the pH value to 2-5, stirring and mixing, and then removing the cationic magnetic microspheres by magnetic separation, filtering, washing and drying to obtain a dried precipitate; S5: crushing and calcining the dried precipitate to obtain Al-doped ZnO low resistivity nanopowder.

[0008] By adopting the above technical solution, since there are many cations on the surface of the cationic magnetic microspheres, they can form chemical adsorption with anions. When the precipitate, the cationic magnetic microspheres and water are stirred and mixed in an environment with a pH value of 2-3, the chemical adsorption stability of the anions and the cationic magnetic microspheres is higher than the physical adsorption of the anions and the precipitate. Therefore, the anions can be dissociated from the precipitate and adsorbed on the surface of the cationic magnetic microspheres, reducing the content of anions in the precipitate, thereby improving the dimensional stability of the Al-doped ZnO low-resistivity nanopowder.

[0009] At the same time, due to the magnetic difference between cationic magnetic microspheres and Al-doped ZnO low resistivity nanopowders, the cationic magnetic microspheres adsorbing anions can be removed by magnetic separation, thereby reducing the residual cationic magnetic microspheres and effectively improving the purity of Al-doped ZnO low resistivity nanopowders.

[0010] Preferably, in S1, the aluminum salt is Al2(SO4)3·18H2O or AlCl3·6H2O.

[0011] Preferably, in S1, the zinc salt is Zn(NO3)2·6H2O or Zn(CH3COO)2·2H2O.

[0012] Preferably, in S1, the molar ratio of aluminum salt to zinc salt is (0.1-0.15):1; In the S2, the molar concentration of the aqueous alkali solution is 1 to 1.2 mol / L.

[0013] By adopting the above technical scheme, the preferred types of aluminum salt and zinc salt are first configured into a reaction precursor solution of a certain concentration according to the above molar ratio, and then an aqueous solution of alkali with a specific molar concentration is added dropwise. The aqueous solution of alkali is mixed more evenly in the reaction precursor solution, which is conducive to refining the aluminum salt and zinc salt, and finally a nano-scale Al-doped ZnO low-resistivity nanopowder is obtained.

[0014] Preferably, in S4, the weight ratio of the precipitate, the cationic magnetic microspheres and water is 1:(0.05-0.24):(5-10).

[0015] By adopting the above technical solution and optimizing the dosage of cationic magnetic microspheres, not only a large amount of anions can be adsorbed, but also they are easy to remove, which is beneficial to reducing the agglomeration of Al-doped ZnO low-resistivity nanopowders and industrial production.

[0016] Preferably, in S4, the method for preparing cationic magnetic microspheres comprises the following steps: A1: stirring and mixing an epoxy silane coupling agent, polyethyleneimine and an organic solvent to obtain a mixture; A2: After the mixture and water are stirred and mixed, silica magnetic microspheres are added, stirred and mixed, filtered, and dried to obtain cationic magnetic microspheres.

[0017] By adopting the above technical solution, since the epoxy group in the epoxysilane coupling agent and the primary amine in the polyethyleneimine can undergo a ring-opening reaction, a mixture containing silicon alkoxy groups and polyethyleneimine segments is obtained. Therefore, after the mixture is mixed with water, the silanol hydrolyzed from the mixture can form hydrogen bonds with the hydroxyl groups on the surface of the silica magnetic microspheres, thereby introducing the polyethyleneimine segments into the surface of the silica magnetic microspheres to obtain cationic magnetic microspheres.

[0018] When the precipitate, cationic magnetic microspheres and water are stirred and mixed at a pH value of 2-3, polyethyleneimine forms a large number of cations on the surface of the magnetic microspheres, which can adsorb a large number of anions, which is beneficial to improving the dimensional stability of the Al-doped ZnO low resistivity nanopowder.

[0019] Preferably, the weight ratio of the silica magnetic microspheres, polyethyleneimine, epoxysilane coupling agent and water is 1:(0.35-0.55):(0.15-0.25):(10-30).

[0020] By adopting the above technical scheme and optimizing the dosage of silica magnetic microspheres, polyethyleneimine and epoxysilane coupling agent in water, the content of cations on the surface of cationic magnetic microspheres can be controlled, which is beneficial to improving the adsorption effect of cationic magnetic microspheres on anions.

[0021] Preferably, the silica magnetic microspheres are mesoporous silica magnetic microspheres with a pore size of 5 to 20 nm.

[0022] By adopting the above technical scheme, the mesoporous silica magnetic microspheres have a highly ordered pore structure, which is conducive to the adsorption of the mixture and increases the grafting amount of polyethyleneimine segments on the surface of the silica magnetic microspheres, thereby further improving the adsorption effect of the cationic magnetic microspheres on anions.

[0023] Preferably, the molecular weight of the polyethyleneimine is 1200-1800, and the viscosity is 3500-15000 MP·s.

[0024] By adopting the above technical scheme, the polyethyleneimine with the above physical properties has a certain solubility and amine functional group, and has good miscibility and reactivity with the epoxy silane coupling agent, which can not only improve the yield of cationic magnetic microspheres, but also the generated cationic magnetic microspheres have a high adsorption capacity for anions.

[0025] Preferably, in S5, the calcination temperature is 850-1000° C., and the calcination time is 8-15 hours.

[0026] By adopting the above technical solution, the precipitate is calcined under the above temperature and time conditions, and the formed grains are not easy to crack. The obtained Al-doped ZnO nanopowder has a good degree of crystallization, a small particle size, a high specific surface area, and excellent conductive properties, and its resistivity can be reduced to 102Ω*cm.

[0027] In summary, this application has the following beneficial effects: 1. Under acidic conditions, the cations formed on the surface of cationic magnetic microspheres can promote the dissociation of anions from the precipitate and form stable chemical adsorption, which reduces the content of anions in the precipitate, effectively reduces the sintering of the precipitate during calcination, and improves the dimensional stability of Al-doped ZnO powder; 2. In the present application, the cationic magnetic microspheres prepared by modifying the silica magnetic microspheres with polyethyleneimine and epoxysilane coupling agents not only have good adsorption to anions, but also have a simple preparation process and low cost; 3. The preparation process of the present application is simple, the equipment requirements are simple, and the Al-doped ZnO nanopowder obtained has high dimensional stability and excellent electrical conductivity, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a SEM image of the Al-doped ZnO nanopowder prepared in Example 1 of the present application; Figure 2 This is a mapping element analysis diagram of Zn element (a), O element (b), and Al element (c) in the Al-doped ZnO nanopowder prepared in Example 1 of the present application; Figure 3 yes Figure 2 Distribution diagram of Zn, O and Al elements. DETAILED DESCRIPTION

[0029] The present application is further described in detail below with reference to the embodiments.

[0030] The raw materials used in the examples of this application are commercially available except for the following special instructions; Epoxy silane coupling agent, brand name KH-560; Silica magnetic microspheres, mesoporous silica magnetic microspheres, model SS-S050JK, purchased from Hangzhou Jikang New Materials Co., Ltd.; The magnetic separator, model CXG-ZN50, was purchased from Shicheng County Guobang Mining Machinery Co., Ltd.

[0031] Preparation Example of Cationic Magnetic Microspheres Preparation Example 1 A cationic magnetic microsphere, each raw material and its corresponding weight (g) are shown in the following table.

[0032] The preparation method of the cationic magnetic microspheres comprises the following steps: A1: The epoxy silane coupling agent, polyethyleneimine and ethanol were stirred and mixed for 20 minutes to obtain a mixture; In the preparation example of the present application, the molecular weight of polyethyleneimine is 1800, the viscosity at 25° C. is 8500-15000 MP·s, the specific gravity is 1.05, and the amine value is 19 mol / g.

[0033] A2: After the mixture and water are stirred for 50 minutes, silica magnetic microspheres are added, stirred for 70 minutes, filtered, and dried to obtain cationic magnetic microspheres.

[0034] Preparation Examples 2-3 A cationic magnetic microsphere, which is different from Preparation Example 1 in that the raw materials and their corresponding weights (g) are shown in the following table.

[0035] Preparation Example 4 A cationic magnetic microsphere, which is different from Preparation Example 1 in that the molecular weight of polyethyleneimine is 1200, the viscosity at 25°C is 3500-7500 MP·s, the specific gravity is 1.05, and the amine value is 19 mol / g.

[0036] Preparation Example 5 A cationic magnetic microsphere, which is different from Preparation Example 1 in that the molecular weight of polyethyleneimine is 10000, the viscosity at 25°C is 40000-150000 MP·s, the specific gravity is 1.04, and the amine value is 18 mol / g.

[0037] Preparation Example 6 A cationic magnetic microsphere, which is different from the preparation example 1 in that the molecular weight of polyethyleneimine is 600, the viscosity at 25°C is 500-2500 MP·s, the specific gravity is 1.05, and the amine value is 20 mol / g.

[0038] Performance Testing The Al-doped ZnO low resistivity nanopowder prepared in the examples and preparation examples of the present application was tested for average particle size, storage stability and water-soluble chloride ion mass fraction. The testing method is as follows: Average particle size: tested according to GB / T13221-2004 standard; Storage stability: Store at room temperature and away from light for 60 days, and visually inspect whether the powder agglomerates; Mass fraction of water-soluble chloride ions: The mass fraction of chloride ions in the powder was determined by the central leaching-potassium thiocyanate volumetric method. Example

[0039] Example 1 An Al-doped ZnO low resistivity nanopowder, the raw materials (g) used in the preparation process and their corresponding weights are shown in the following table.

[0040] The method for preparing the Al-doped ZnO low-resistivity nanopowder comprises the following steps: S1: stirring and mixing aluminum salt, zinc salt and water to obtain a reaction precursor solution; In the embodiments of the present application, the aluminum salt is AlCl3·6H2O and the zinc salt is Zn(NO3)2·6H2O.

[0041] S2: adding the aqueous solution of alkali dropwise into the reaction precursor solution, stirring and mixing for 1 hour to obtain a sol solution; In the embodiment of the present application, the alkali in the aqueous alkali solution is sodium hydroxide.

[0042] S3: centrifuging the sol solution to obtain a precipitate; S4: After mixing the precipitate, cationic magnetic microspheres and water, the pH value is adjusted to 3, and after stirring and mixing for 30 minutes, a magnetic separator is used to remove the cationic magnetic microspheres, and then the mixture is washed with anhydrous ethanol for 3 times, and finally dried at 100°C for 24 hours to obtain a dried precipitate; In the examples of the present application, the cationic magnetic microspheres are the cationic magnetic microspheres prepared in Preparation Example 1.

[0043] S5: The dried precipitate is crushed at a rotation speed of 10000 r / min for 5 minutes, and then calcined at 900° C. for 10 hours to obtain Al-doped ZnO low resistivity nanopowder.

[0044] Example 2 An Al-doped ZnO low resistivity nanopowder is different from Example 1 in that in the preparation methods S1 and S2 of the Al-doped ZnO low resistivity nanopowder, the raw materials used in the preparation process and their corresponding weights (g) are shown in the following table.

[0045] In the embodiments of the present application, the aluminum salt is AlCl3·6H2O and the zinc salt is Zn(NO3)2·6H2O.

[0046] Example 3 An Al-doped ZnO low resistivity nanopowder is different from Example 1 in that in the preparation methods S1 and S2 of the Al-doped ZnO low resistivity nanopowder, the raw materials used in the preparation process and their corresponding weights (g) are shown in the following table.

[0047] In the embodiments of the present application, the aluminum salt is AlCl3·6H2O and the zinc salt is Zn(CH3COO)2·2H2O.

[0048] The average particle size, storage stability and mass fraction of water-soluble chloride ions of the Al-doped ZnO low-resistivity nanopowders prepared in Examples 1 to 3 of the present application were tested, and the test results are shown in the following table.

[0049] Depend on Figure 1 It can be seen that in Example 1, the Al-doped ZnO powder presents a spherical structure after calcination, and the average particle size is about 200 nm. Due to the high calcination temperature, the spherical powder is closely arranged and has a clear edge contour.

[0050] Depend on Figure 2 , 3 It can be seen that in Example 1, the Al-doped ZnO powder contains Al, Zn, and O, wherein the content of Al is below 10%, indicating that the main body of the sample powder is ZnO, and the rest is a small amount of aluminum oxide doping.

[0051] By analyzing the data in the above table, it can be seen that the Al-doped ZnO low-resistivity nanopowder prepared in Examples 1 to 3 has an average particle size in the range of 218 to 256 nm, a water-soluble chloride ion mass fraction as low as 43 to 50 ppm, and no agglomeration occurs after storage at room temperature for 60 days. This shows that the Al-doped ZnO low-resistivity nanopowder prepared in Examples 1 to 3 of the present application has good dimensional stability.

[0052] Embodiment 4-5 An Al-doped ZnO low-resistivity nanopowder is different from Example 1 in that, in the preparation method S4 of the Al-doped ZnO low-resistivity nanopowder, the raw materials used in the preparation process and their corresponding weights (g) are shown in the following table.

[0053] The mass fraction of water-soluble chloride ions was detected for the Al-doped ZnO low resistivity nanopowders prepared in Examples 1, 4 to 5 of the present application. The test results are shown in the following table.

[0054] By analyzing the data in the above table, it can be seen that the water-soluble chloride ion mass fraction of the Al-doped ZnO low-resistivity nanopowder prepared in Examples 1, 4-5 is as low as 43-68 ppm, wherein the water-soluble chloride ion mass fraction of Example 1 is similar to that of Example 5. This shows that in the preparation method of the Al-doped ZnO low-resistivity nanopowder of the present application, when the weight ratio of the precipitate, the cationic magnetic microspheres and water is 1:(0.05-0.24):(5-10), not only a large amount of anions can be adsorbed, but also the amount of cationic magnetic microspheres used is small and easy to remove.

[0055] Embodiments 6 to 10 An Al-doped ZnO low resistivity nano powder, which is different from Example 1 in that the cationic magnetic microspheres are prepared using the cationic magnetic microspheres prepared by the preparation examples in the following table. Example Preparation Example of Cationic Magnetic Microspheres Example 6 Preparation Example 2 Example 7 Preparation Example 3 Example 8 Preparation Example 4 Example 9 Preparation Example 5 Example 10 Preparation Example 6

[0056] The Al-doped ZnO low resistivity nanopowders prepared in Examples 1, 6 to 10 of the present application were tested for water-soluble chloride ion mass fraction and storage stability. The test results are shown in the following table.

[0057] By analyzing the data in the above table, it can be seen that the water-soluble chloride ion mass fraction of the Al-doped ZnO low-resistivity nanopowder prepared in Examples 1, 6 to 7 is as low as 46 to 63 ppm, among which the water-soluble chloride ion mass fraction of Example 1 is the lowest. This shows that in the preparation method of the Al-doped ZnO low-resistivity nanopowder of the present application, when the weight ratio of silica magnetic microspheres, polyethyleneimine, epoxysilane coupling agent and water is 1: (0.35 to 0.55): (0.35 to 0.55): (10 to 30), the cationic magnetic microspheres have a good adsorption effect on anions, which can effectively improve the dimensional stability of the Al-doped ZnO low-resistivity nanopowder. The reason for this may be that by optimizing the amount of silica magnetic microspheres, polyethyleneimine and epoxysilane coupling agent in water, the content of cations on the surface of the cationic magnetic microspheres can be controlled, thereby improving the adsorption effect of the cationic magnetic microspheres on anions.

[0058] At the same time, the Al-doped ZnO low-resistivity nanopowder prepared in Examples 1 and 8 has a water-soluble chloride ion mass fraction as low as 46 to 52 ppm. Compared with Examples 9 and 10, Examples 1 and 8 have a lower water-soluble chloride ion mass fraction. This shows that in the preparation method of the Al-doped ZnO low-resistivity nanopowder of the present application, the cationic magnetic microspheres prepared by polyethyleneimine with a molecular weight of 1200 to 1800 and a viscosity of 3500 to 15000 MP·s are used for treatment, which can reduce the chloride ion content in the Al-doped ZnO low-resistivity nanopowder and improve the dimensional stability of the Al-doped ZnO low-resistivity nanopowder.

[0059] Embodiment 11 An Al-doped ZnO low-resistivity nanopowder, which is different from Example 1 in that a method for preparing the Al-doped ZnO low-resistivity nanopowder comprises the following steps: S1: The same as in Example 1, to obtain a reaction precursor solution.

[0060] S2: The same as Example 1, to obtain a sol solution.

[0061] S4: After mixing the precipitate, cationic magnetic microspheres and water, adjust the pH value to 2, stir and mix for 25 minutes, first use a magnetic separator to remove the cationic magnetic microspheres, then wash with anhydrous ethanol for 3 times, and finally dry at 100°C for 24 hours to obtain a dried precipitate.

[0062] S5: The dried precipitate is crushed at a rotation speed of 10000 r / min for 5 minutes, and then calcined at 600° C. for 20 hours to obtain Al-doped ZnO low resistivity nanopowder.

[0063] Example 12 An Al-doped ZnO low-resistivity nanopowder, which is different from Example 1 in that a method for preparing the Al-doped ZnO low-resistivity nanopowder comprises the following steps: S1: The same as in Example 1, to obtain a reaction precursor solution.

[0064] S2: The same as Example 1, to obtain a sol solution.

[0065] S4: After mixing the precipitate, cationic magnetic microspheres and water, adjust the pH value to 5, stir and mix for 40 minutes, first use a magnetic separator to remove the cationic magnetic microspheres, then wash with anhydrous ethanol for 3 times, and finally dry at 100°C for 24 hours to obtain a dried precipitate.

[0066] S5: The dried precipitate is crushed at a rotation speed of 10000 r / min for 5 minutes, and then calcined at 1050° C. for 5 hours to obtain Al-doped ZnO low resistivity nanopowder.

[0067] The Al-doped ZnO low resistivity nanopowders prepared in Examples 1, 11, and 12 of the present application were tested for storage stability and water-soluble chloride ion mass fraction. The test results are shown in the following table.

[0068] By analyzing the data in the above table, it can be seen that the Al-doped ZnO low-resistivity nanopowder prepared in Examples 1, 11, and 12 has a water-soluble chloride ion mass fraction as low as 46 to 54 ppm, and no agglomeration occurs after storage at room temperature for 60 days. This shows that in the preparation method of the Al-doped ZnO low-resistivity nanopowder of the present application, the cationic magnetic microspheres have a good adsorption effect on the anions in the precipitate under an environment of pH 2 to 5, and in particular, the cationic magnetic microspheres have the best adsorption effect on the anions in the precipitate under an environment of pH 3 and stirring and mixing for 30 minutes.

[0069] Embodiments 13-14 An Al-doped ZnO low resistivity nanopowder is different from Example 1 in that in the preparation methods S1 and S2 of the Al-doped ZnO low resistivity nanopowder, the weight (g) of each raw material used in the preparation process is shown in the following table.

[0070] The average particle size and storage stability of the Al-doped ZnO low resistivity nanopowders prepared in Examples 1, 13, and 14 of the present application were tested, and the test results are shown in the following table.

[0071] By analyzing the data in the above table, it can be seen that the average particle size of the Al-doped ZnO low-resistivity nanopowder prepared in Example 1 is lower than that of the Al-doped ZnO low-resistivity nanopowder prepared in Examples 13 and 14. This shows that in the preparation method of Al-doped ZnO low-resistivity nanopowder, when in S1, the aluminum salt is Al2(SO4)3·18H2O or AlCl3·6H2O; the zinc salt is Zn(NO3)2·6H2O or Zn(CH3COO)2·2H2O; and the molar ratio of the aluminum salt to the zinc salt is (0.1-0.15):1, the average particle size of the Al-doped ZnO low-resistivity nanopowder can be reduced.

[0072] Comparative Example Comparative Example 1 An Al-doped ZnO low-resistivity nanopowder, which is different from Example 1 in that a method for preparing the Al-doped ZnO low-resistivity nanopowder comprises the following preparation steps: S1: stirring and mixing aluminum salt, zinc salt and water to obtain a reaction precursor solution; S2: adding the aqueous solution of alkali dropwise into the reaction precursor solution, stirring and mixing for 1 hour to obtain a sol solution; S3: centrifuging the sol solution to obtain a precipitate; S4: washing the precipitate with anhydrous ethanol for three times, and finally drying it at 100° C. for 24 h to obtain a dried precipitate; S5: The dried precipitate is crushed at a rotation speed of 10000 r / min for 5 minutes, and then calcined at 900° C. for 10 hours to obtain Al-doped ZnO low resistivity nanopowder.

[0073] The average particle size, storage stability and mass fraction of water-soluble chloride ions of the Al-doped ZnO low resistivity nanopowder prepared in Example 1 and Comparative Example 1 of the present application were tested, and the test results are shown in the following table.

[0074] By analyzing the data in the above table, it can be seen that compared with Example 1, the average particle size of the Al-doped ZnO low-resistivity nanopowder prepared in Comparative Example 1 is significantly increased, agglomeration occurs after 60 days of storage at room temperature, and the mass fraction of water-soluble chloride ions is as high as 3500ppm. This shows that in the preparation method of the Al-doped ZnO low-resistivity nanopowder of the present application, cationic magnetic microspheres and precipitates are stirred and mixed in water with a pH value of 2 to 5, and the cationic magnetic microspheres can adsorb anions in the precipitate, thereby improving the removal rate of anions in the Al-doped ZnO low-resistivity nanopowder, reducing the salt bridge of anions during calcination, thereby improving the dimensional stability of the Al-doped ZnO low-resistivity nanopowder.

[0075] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for preparing Al-doped ZnO low resistivity nanopowder, characterized in that: The method comprises the following preparation steps: S1: stirring and mixing aluminum salt, zinc salt and water to obtain a reaction precursor solution; S2: adding the aqueous solution of alkali dropwise into the reaction precursor solution, stirring and mixing, to obtain a sol solution; S3: centrifuging the sol solution to obtain a precipitate; S4: after mixing the precipitate, cationic magnetic microspheres and water, adjusting the pH value to 2-5, stirring and mixing, and then removing the cationic magnetic microspheres by magnetic separation, filtering, washing and drying to obtain a dried precipitate; S5: crushing and calcining the dried precipitate to obtain Al-doped ZnO low resistivity nanopowder.

2. The method for preparing Al-doped ZnO low resistivity nanopowder according to claim 1, characterized in that: In the S1, the aluminum salt is Al2(SO4)3•18H2O or AlCl3•6H2O.

3. The method for preparing Al-doped ZnO low resistivity nanopowder according to claim 1, characterized in that: In the S1, the zinc salt is Zn(NO3)2•6H2O or Zn(CH3COO)2•2H2O.

4. The method for preparing Al-doped ZnO low resistivity nanopowder according to claim 1, characterized in that: In S1, the molar ratio of aluminum salt to zinc salt is (0.1-0.15):

1.

5. The method for preparing Al-doped ZnO low resistivity nanopowder according to claim 1, characterized in that: In the S4, the weight ratio of the precipitate, the cationic magnetic microspheres and water is 1:(0.05-0.24):(5-10).

6. The method for preparing Al-doped ZnO low resistivity nanopowder according to claim 1, characterized in that: In S4, the preparation method of cationic magnetic microspheres comprises the following steps: A1: stirring and mixing an epoxy silane coupling agent, polyethyleneimine and an organic solvent to obtain a mixture; A2: After the mixture and water are stirred and mixed, silica magnetic microspheres are added, stirred and mixed, filtered, and dried to obtain cationic magnetic microspheres.

7. The method for preparing Al-doped ZnO low resistivity nanopowder according to claim 6, characterized in that: The weight ratio of the silica magnetic microspheres, polyethyleneimine, epoxysilane coupling agent and water is 1:(0.35-0.55):(0.25-0.35):(10-30).

8. The method for preparing Al-doped ZnO low resistivity nanopowder according to claim 7, characterized in that: The silica magnetic microspheres are mesoporous silica magnetic microspheres with a pore size of 5 to 20 nm.

9. The method for preparing Al-doped ZnO low resistivity nanopowder according to claim 5, characterized in that: The molecular weight of the polyethyleneimine is 1200-1800, and the viscosity is 3500-15000 MP•s.

10. The method for preparing Al-doped ZnO low resistivity nanopowder according to claim 1, characterized in that: In the step S5, the calcination temperature is 600 to 1050° C., and the calcination time is 5 to 20 hours.