Embodiment 1
[0053] Washable floor and wall paint, consisting of the following raw materials in parts by mass:
[0054] 78.6 parts of water,
[0055] 6.0 parts of polyvinyl alcohol,
[0056] 0.3 parts of hydroxyethyl cellulose,
[0057] 2 parts of propylene glycol,
[0058] 2 parts glycerol,
[0059] Talcum powder 2 parts,
[0060] Calcium carbonate 2 parts,
[0061] 4 parts of 3M hollow glass microspheres K20,
[0062] Fluorescent pink powder AX-11 3 parts,
[0063] Preservative Casson 0.1 parts.
[0064] Weigh the above-mentioned raw materials respectively by weight, first add 6 parts of polyvinyl alcohol into 34 parts of water, heat up to about 90 degrees, until the polyvinyl alcohol is completely dissolved, add the remaining 44.6 parts of water after cooling, start stirring, Add the weighed raw materials one by one according to the above raw material sequence from front to back. When the added raw materials are in powder form, adjust the stirring speed to 1000rpm and disperse a...
Embodiment 2
[0066]A kind of washable floor and wall paint, composed of the following raw materials in parts by mass:
[0067] 75.9 parts of water,
[0068] 2.5 parts of polyvinyl alcohol,
[0069] 1 part hydroxyethyl cellulose,
[0070] 3 parts of propylene glycol,
[0071] 3 parts of glycerol,
[0072] 3.5 parts of talcum powder,
[0073] 3.5 parts of calcium carbonate,
[0074] 4 parts of 3M hollow glass microspheres K20,
[0075] Fluorescent orange powder AX-15 3.5 parts,
[0076] Preservative Casson 0.1 parts.
[0077] Weigh the above-mentioned raw materials respectively by weight, first add 2.5 parts of polyvinyl alcohol to 16.66 parts of water, heat up to about 90 degrees, until the polyvinyl alcohol is completely dissolved, add the remaining 59.24 parts of water after cooling, start stirring, Add the weighed raw materials one by one according to the above raw material sequence from front to back. When the added raw materials are in powder form, adjust the stirring speed to ...
Embodiment 3
[0079] A kind of washable floor and wall paint, composed of the following raw materials in parts by mass:
[0080] 67.06 parts of water,
[0081] Polyvinylpyrrolidone PVP-K30 3 parts,
[0082] 7 parts polyacrylic acid,
[0083] 0.34 parts of neutralizing agent sodium hydroxide,
[0084] 3 parts of propylene glycol,
[0085] 3 parts of glycerol,
[0086] 4 parts talcum powder,
[0087] 4 parts calcium carbonate,
[0088] 5 parts of 3M hollow glass microspheres K20,
[0089] Fluorescent yellow powder AX-17 3.5 parts,
[0090] Preservative Casson 0.1 parts.
[0091] Weigh the above raw materials in parts by weight, first add 3 parts of polyvinylpyrrolidone PVP-K30 to 67.06 parts of water, raise the temperature to about 90 degrees, until the PVP-K30 is completely dissolved, start stirring, and follow the above-mentioned sequence of raw materials from front to back Add the weighed raw materials one by one (the neutralizer sodium hydroxide is not added first), when the adde...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com