A kind of method that prepares hot-melt adhesive by lac waste slag glue and waste polyester

A technology of waste polyester and waste slag, which is applied in the direction of adhesives, etc., can solve the problems of long preparation process, waste of resources, and increased costs, and achieve the effects of reducing manufacturing costs, improving fluidity, and reducing emissions

CN108997586BActive Publication Date: 2020-11-17KUNMING UNIV OF SCI & TECH
12 Cites 0 Cited by

Patent Information

Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Publication Date
2020-11-17

Smart Images

  • Figure 1
    Figure 1
  • Figure 2
    Figure 2
  • Figure 3
    Figure 3
Patent Text Reader

Abstract

The invention discloses a method for preparing hot melt adhesive from lac waste residue glue and waste polyester. The method comprises the following steps: (1) treating the ac waste residue glue; (2)treating the waste polyester; (3) performing alcoholysis reaction on the waste polyester and diol; (4) performing co-grafting / coupling reaction on the waste polyester alcoholysis product, the lac waste residue glue, polymerized rosin glycidyl ester and glycidyl rosin; and (5) adding other additives, mixing and discharging. According to the prepared hot melt adhesive, the softening point is between99 and 120 DEG C, MFR is between 20 and 44 g / 10min and the shear strength is between 4.6 and 5.6 MPa; and the hot melt adhesive has a low melting point, high flowability and high bonding strength andcan meet the use requirement on hot bonding of materials such as wood, and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field

[0001] The present invention relates to a method of preparing hot melt glue from a purple polyester, particularly with low softening points and high fluidity, suitable for wood and carton hot melt bonding. And the method of preparing a hot melt glue, belonging to the abutment of the polyester. Background technique

[0002] The hot melt glue is heated, and the adhesive that achieves bonding is quickly solidified at room temperature. Since it does not contain any solvent, non-toxic, odorless, non-polluted environment, is known as "green adhesive", and thus has a wide range of applications in all walks of life. The polyester hot melt adhesive appeared in the 1960s, polyester for hot melt glue is a saturated polyester resin, which has a certain crystallinity, rigidity, and toughness, excellent electrical energy, water resistance, heat resistance. , Cold-resistant and medium resistance, and high viscosity, bonding a variety of materials, widely used in clothing, automo...

Examples

Embodiment 1

[0059] Gum lac and discarding waste slag preparation polyester hot-melt adhesive, a raw material which comprises: dehydrating waste slag shellac gum 20g, waste PET 100g, 20g of ethylene glycol (ethylene glycol / polyester waste is 0.6 molar ratio), zinc acetate 0.7g, glycidyl ester of polymerized rosin, 10g, glycidyl ester of rosin 15g, tackifying resins 13.2g [(3) ~ (4) step 8% of the total feeding amount], light calcium carbonate 13.2g [(3) - step (4) the total feeding amount of 8%], antioxidant 1010 0.33g [(3) ~ (4) step total feeding amount of 0.2%]. Preparation of Hot Melt specific steps are as follows:

[0060] Preparation of (1) dehydration of waste slag shellac gum

[0061] Extracted from the gum or shellac particles shellac gum production line made aleuritic acid residue discarded gum shellac, a vacuum oven at 85 ℃ 8h remove water and dried in vacuo to prepare a dehydrated waste slag shellac gum, referred to as WS. Black viscous liquid at room temperature (melting point l...

Embodiment 2

[0074] Gum lac and discarding waste slag preparation polyester hot-melt adhesive, a raw material which comprises: dehydrating waste slag shellac gum 50g, waste PET 100g, 30g of ethylene glycol (ethylene glycol / polyester waste is 0.9 molar ratio), manganese acetate 1.2g, 13g glycidyl ester of polymerized rosin, rosin glycidyl 7g, tackifying resins 20.1g [(3) ~ (4) step total feeding amount of 10%], light calcium carbonate 20.1g [(3) - step (4) the total feeding amount of 10%], antioxidant 0.80g [(3) ~ (4) step total feeding amount of 0.4%].

[0075] Specifically Step 1, except that the same Example:

[0076] Step (1) was dried in vacuo at 78 deg.] C 12h;

[0077] Step (4) the grafting of CPC / coupling reaction temperature was 180 ℃, the reaction time is 2H;

[0078] Step (5) The mixture was poured into hot water of 40 ℃.

[0079] The hot melt adhesive was measured softening point of 112 ℃, MFR of 31g / 10min, the shear strength of 5.1MPa.

Embodiment 3

[0081] Gum lac and discarding waste slag preparation polyester hot-melt adhesive, a raw material which comprises: dehydrating waste slag shellac gum 70g, waste PET 100g, 4Og glycol (ethylene glycol / polyester waste is 1.2 molar ratio), zinc acetate 1.0g, glycidyl ester of polymerized rosin, 16g, glycidyl ester of rosin 10g, tackifying resins 28.4g [(3) ~ (4) step total feeding amount of 12%], light calcium carbonate 28.4g [(3) - step (4) the total feeding amount of 12%], antioxidant 1.42g [(3) ~ (4) step total feeding amount of 0.6%].

[0082] Specifically Step 1, except that the same Example:

[0083] Step (1) was dried in vacuo for 16h 70 ℃;

[0084] Step (4) the grafting of CPC / coupling reaction temperature was 170 ℃, the reaction time is 3H;

[0085] Step (5) The mixture was poured into hot water of 50 deg.] C.

[0086] The hot melt adhesive was measured softening point of 106 ℃, MFR of 35g / 10min, the shear strength of 5.6MPa.

[0087] Wherein the step of black viscous liqu...