High-temperature brazing alloy welding flux for ceramic and steel welding and its preparing method

A brazing alloy and high-temperature technology, which is applied in the fields of carbon, brazing material for high-temperature working ceramic tools, nitride ceramics and steel welding, can solve the problems of low high-temperature strength, short service life and high cost of brazing joints, and achieve brazing Good weld performance, high mechanical properties, and good formability

Inactive Publication Date: 2008-12-10
HUAZHONG UNIV OF SCI & TECH
View PDF6 Cites 1 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

But the price is expensive (150 yuan / Kg), and the high temperature strength of brazed joints is relatively low (<200MPa)
Therefore, when brazing ceramic tools that need to work in high temperature environment, it will lead to high cost and short service life

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • High-temperature brazing alloy welding flux for ceramic and steel welding and its preparing method
  • High-temperature brazing alloy welding flux for ceramic and steel welding and its preparing method

Examples

Experimental program
Comparison scheme
Effect test

preparation example Construction

[0013] The preparation method of the present invention is as follows:

[0014] (1) slowly heating the nickel ingot to 1500-1550°C in a vacuum induction furnace;

[0015] (2) After the nickel ingot is completely melted, add the niobium ingot and keep warm so that the niobium is completely dissolved into the nickel solution;

[0016] (3) Lower the temperature of the above-mentioned Ni-Nb liquid alloy to 1400-1450 ° C, then add copper ingots, keep warm until the copper is completely dissolved in the Ni-Nb liquid alloy to make its composition uniform, and then reduce the temperature of the alloy melt to 1300-1350℃;

[0017] (4) Forming is performed to obtain solder in a desired shape.

[0018] It can be processed and shaped by milling, drawing, rolling and other methods. When making powder, use the argon atomization method to atomize the metal liquid into fine powder with high-pressure argon, collect, cool, and sieve into powder solder with a particle size of less than 150 mesh...

Embodiment 1

[0020] Prepare materials with 30wt% Cu, 20wt% Nb, and the rest as Ni, and smelt them in a vacuum induction furnace. When smelting, first heat the nickel ingots to 1500°C to melt (called "melting temperature"), and then add niobium ingots. After the niobium ingot is cleared, lower the temperature to 1400°C (called "copper addition temperature"), then add the copper ingot into the Ni-Nb liquid alloy, and keep warm until the copper is completely dissolved in the Ni-Nb liquid alloy, so that Its composition is uniform, and then the temperature of the alloy melt is lowered to 1300°C (called "casting temperature"), and then poured into 100×100×200mm 3 of ingots. After the ingot is heated to 800-1000°C, it is upsetting and elongated with a 120-ton air hammer, and finally made into 10×50×400mm 3 10 pieces of slabs. Heat the slab to 950°C for 30 minutes, quickly cool it in oil for solution treatment, and then make a 0.5mm thick plate-shaped brazing material to braze Ti(C,N) ceramics a...

Embodiment 2

[0022] Prepare materials with 35wt% Cu, 23wt% Nb, and the rest as Ni, and smelt in a vacuum induction furnace. The smelting process is the same as in Example 1. The melting temperature is 1530°C, the copper addition temperature is 1420°C, and the casting temperature is 1320°C. Then make 180-mesh powdered brazing material, braze the TiC-based ceramic blade and 40Cr steel, polish the surface to be welded to a mirror surface before welding, and clean it with 30-40% HCl aqueous solution, then further clean it with acetone, and dry it. Brazing is performed directly in a cold-wall vacuum furnace. The brazing specification is the same as in Example 1, and the obtained brazed joint has good mechanical properties, the bending strength at room temperature is 1600-1700MPa, the bending strength at 600°C is 1000-1100MPa, the brazing seam is flat, and there is no oxidation phenomenon.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
flexural strengthaaaaaaaaaa
flexural strengthaaaaaaaaaa
flexural strengthaaaaaaaaaa
Login to View More

Abstract

The present invention discloses an alloy soldering flux for high-temperature soldering ceramics and steel, and its preparation method. The composition of said soldering flux contains (by wt%) 20-25% of Nb, 30-40% of Cu and the rest is Ni. Its preparation method includes the following steps: heating the nickel ingot to 1500-1550 deg.C in vacuum induction furnace, after the nickel ingot is completely molten, adding niobium ingot, heat-insulating to make the niobium ingot be dissolved in molten nickel, cooling Ni-Nb liquid alloy to 1400-1450 deg.C, then adding copper ingot, heat-insulating to make the copper ingot be completely dissolved in Ni-Nb liquid alloy, uniformly mixing them, cooling to 1300-1350 deg.C, finally forming so as to obtain the invented product.

Description

technical field [0001] The invention belongs to the field of welding technology, and relates to a brazing material for high-temperature working ceramic tools, which is especially suitable for welding carbon and nitride ceramics and steel. Background technique [0002] At present, there are generally two methods for welding ceramics and steel in the world. One is metallization of the ceramic surface (the so-called MnMo method), and then brazing with the metal. The other is direct brazing with active solder. After 1980, most of the brazing of ceramic and metal structural parts used active solder. The solder used is silver-copper-titanium alloy. The characteristics of silver-copper-titanium series brazing material are: relatively low melting point 950-1050 ℃, strong wetting ability to ceramics, and high strength of room temperature brazing joints. But the price is expensive (150 yuan / Kg), and the high-temperature strength of the brazed joint is relatively low (<200MPa). ...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & AuthorityPatents(China)
IPC IPC(8): B23K35/30C22C1/02
Inventor周世权赵卫周文祺
OwnerHUAZHONG UNIV OF SCI & TECH