Method for joint production of titanium/titanium alloy strip by short-process four-high and twenty-high rolling mills
A joint production, titanium alloy technology, applied in the direction of rolling mill control device, roll, roll speed control, etc., can solve the problem of undiscovered reports, and achieve the effect of reducing production cost, improving yield and good quality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0022] To produce ultra-fine-grained extremely thin titanium (TA1) ribbons with a thickness of 0.3 mm, prepared by the following steps:
[0023] (1) Completely anneal the titanium / titanium alloy coil with a thickness of 3.15mm and a width of 800mm produced by the hot rolling mill, the annealing temperature is 800°C, and the annealing time is 220min;
[0024] (2) Shot blast the titanium / titanium alloy strip after the annealing is completed, pickling after the shot blasting, and coiling after the pickling;
[0025] (3) The roughness of the work roll surface of the four-roll mill is controlled at 60~65 mesh, the coolant of the four-roll mill is cooled by a large amount of oil, and the first rolling pass adopts low pressure reduction and low rolling speed Carry out hot rolling, the amount of low pressure is that the deformation is 11% of the base material, and the low rolling speed is that the rolling speed does not exceed 10m / min. After the hot rolling is completed, four passes a...
Embodiment 2
[0032] Production of ultra-fine-grained ultra-thin titanium alloy strips (TA10) with a thickness of 0.2mm, prepared by the following steps:
[0033] (1) Completely anneal the TA10 titanium alloy coil with a thickness of 3.0mm and a width of 400mm produced by the hot rolling mill. The annealing temperature is 850°C and the annealing time is 180min;
[0034] (2) Shot blast the TA10 titanium alloy strip after the annealing is completed, pickling after the shot blasting, and coiling after the pickling;
[0035] (3) The roughness of the work roll surface of the four-high rolling mill is controlled at 65 mesh, and the coolant of the four-high rolling mill is cooled by a large amount of oil. Roll, the amount of low-pressure reduction is that the deformation is 12% of the base material, and the low rolling speed is that the rolling speed does not exceed 10m / min. After the hot roll is completed, the titanium / titanium alloy strip is rolled to 0.65mm in 5 passes. The deformation rate is...
PUM
| Property | Measurement | Unit |
|---|---|---|
| thickness | aaaaa | aaaaa |
| thickness | aaaaa | aaaaa |
| thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More 