[0047] Example 1: A gelled powder with negative ion biomimetic function
[0048] 1. Formula composition (substances are measured in parts by weight):
[0049] (1) 41 parts of natural β-calcium sulfate hemihydrate;
[0050] (2) Diatomite: 12 parts of ground diatomite powder with a particle size of 400-800 mesh;
[0051] (3) Inorganic environmental minerals: 4 parts of seagull stone powder
[0052] (4) Modifier: 2 parts of compound powder uniformly mixed with 54% calcium oxide, 36% silicon oxide and 10% polyvinyl alcohol;
[0053] 2. Production and preparation process:
[0054] (1) Pretreatment of raw materials: β-calcium sulfate hemihydrate, diatomaceous earth, seagull stone powder, and modifiers are accurately measured according to 41 parts, 12 parts, 4 parts, and 2 parts respectively;
[0055] (2) After pre-mixing, it is prepared by aging in an aging warehouse for 3-15 days.
Embodiment 2
[0056] Embodiment 2: A kind of decorative plate with negative ion bionic function
[0057] 1. Formula composition (substances are measured in parts by weight):
[0058] (1) 47.8 parts of calcium phosphate;
[0059] (2) Diatomite: 10 parts of ground diatomite powder with a particle size of 400-800 mesh;
[0060] (3) Inorganic environmental minerals: 2 parts of seagull stone powder
[0061] (4) Modifier: 2 parts of compound powder uniformly mixed with 60% calcium oxide, 32% silicon oxide and 8% polyvinyl alcohol;
[0062] (5) Reinforced fiber chopped strands: 0.2 parts of glass fiber with a length of 18-20mm;
[0063] (6) Composite solution: clear water, crystal modifier, waterproofing agent, and defoamer are mixed and stirred according to their mass ratio of 100:1.8:0.4:0.5 to form 38 parts of a uniform composite solution; the crystal modifier is Sodium citrate; The waterproofing agent is sodium methyl siliconate; The defoamer is tributyl phosphate.
[0064] 2. Production ...
Embodiment 3
[0070] Embodiment 3: A kind of filler with negative ion biomimetic function
[0071] 1. Formula composition (substances are measured in parts by weight):
[0072] (1) 47 parts of calcium aluminate;
[0073] (2) Seaweed earth: 8 parts of seaweed earth powder with a particle size of 400-800 mesh and ground;
[0074] (3) Inorganic environmental minerals: 6 parts of tourmaline powder
[0075] (4) Modifier: 2 parts of compound powder uniformly mixed with 54% calcium oxide, 36% silicon oxide and 10% polyvinyl alcohol;
[0076] (5) Reinforced fiber chopped strands: 1.0 parts of mineral fiber with a length of 8-12 mm;
[0077] (6) Composite solution: clear water, crystal modifier, waterproofing agent, and defoamer are mixed and stirred according to their mass ratio of 100:1.8:0.4:0.5 to form 36 parts of a uniform composite solution; the crystal modifier is Aluminum potassium sulfate; Described waterproof agent is siloxane; Described defoamer is isoamyl alcohol.
[0078] 2. Produc...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
length | aaaaa | aaaaa |
length | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com