High-gloss water-based paint for perfume glass bottles
A water-based paint and glass bottle technology, applied in the direction of anti-corrosion paint, coating, etc., can solve the problems of affecting the production line capacity, increasing the process, poor alcohol resistance, etc., to increase the fullness of the paint film, increase the solid content of the paint, and excellent durability chemical effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0049] According to the following preparation method, according to the formula shown in the following table 1, the high-gloss water-based coating for the perfume glass bottle is prepared:
[0050] Component A: Add acrylic resin A to acrylic resin B under slow stirring, stir at a stirring speed of 1000 rpm for 15 minutes, add co-solvent and deionized water, and adjust the pH value to 8. Then add melamine resin A, melamine resin B, defoamer, and leveling agent to the stirring mixture in sequence, stir at medium speed (1500 rpm) for 30 minutes, add defoamer, and disperse at high speed (2000 rpm) for 30 minutes , then add an amine neutralizer to adjust the pH value to 8, stir at a medium speed (1500 rpm) for 15 minutes, use a rheological additive to adjust the product viscosity, let it stand overnight, add a silane coupling agent, and use an amine neutralizer again Adjust the pH value to 8, adjust the viscosity with a rheological additive or deionized water, filter with a 400-mesh...
Embodiment 2
[0060] According to the following preparation method, according to the formula shown in the following table 2, the high-gloss water-based coating for the perfume glass bottle is prepared:
[0061] Component A: Add acrylic resin A to acrylic resin B under slow stirring. After stirring for 20 minutes, add co-solvent and deionized water. After stirring evenly, adjust the pH value to 8.5 with amine neutralizer, and then add Melamine resin A, melamine resin B, defoamer, leveling agent, stir at medium speed (1500 rpm) for 30 minutes, add defoamer, disperse at high speed (2000 rpm) for 30 minutes, then add amine neutralizer to adjust PH When the value reaches 8.5, stir at a medium speed (1500 rpm) for 15 minutes, adjust the viscosity of the product with a rheological additive, let it stand overnight, add a silane coupling agent, adjust the pH value to 8.5 with an amine neutralizer again, and use a rheological additive to adjust the pH value to 8.5. Auxiliary or deionized water to adj...
PUM
Property | Measurement | Unit |
---|---|---|
density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com