Fluid loss reducer with core-shell structure, preparation method and application thereof, and water-based drilling fluid

A technology of fluid loss control agent and core-shell structure, which is applied in the field of fluid loss control agent for water-based drilling fluid and water-based drilling fluid. Achieve the effects of improved temperature resistance, environmental friendliness and low cost

Active Publication Date: 2022-03-22
CHINA UNIV OF PETROLEUM (EAST CHINA)
View PDF0 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] The purpose of the present invention is to solve the problem of insufficient temperature resistance, salt resistance and anti-calcium performance of the fluid loss control agent for water-based drilling fluid, to provide a fluid loss control agent with a core-shell structure and its preparation method and application and water-based drilling fluid

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Fluid loss reducer with core-shell structure, preparation method and application thereof, and water-based drilling fluid
  • Fluid loss reducer with core-shell structure, preparation method and application thereof, and water-based drilling fluid
  • Fluid loss reducer with core-shell structure, preparation method and application thereof, and water-based drilling fluid

Examples

Experimental program
Comparison scheme
Effect test

preparation example Construction

[0020] The first aspect of the present invention provides a method for preparing a fluid loss control agent with a core-shell structure, the method comprising the following steps:

[0021] (1) Solvent, emulsifier-1 and co-emulsifier are mixed to obtain continuous phase;

[0022] (2) aqueous solution containing multiple polymer monomers, emulsifier-2, calcium chloride, sodium carbonate and silane coupling agent are prepared into suspension;

[0023] (3) mixing the suspension and the continuous phase into an emulsion;

[0024] (4) Reacting the emulsion in the presence of an oxidant and a reducing agent, and the obtained product is subjected to demulsification, filtration, filter cake washing and drying to obtain the fluid loss control agent.

[0025] In some embodiments of the present invention, preferably, in the continuous phase, the amount of the emulsifier-1 is 5-15% w / v of the volume of the solvent, that is, relative to 100 mL of the solvent, the The amount of emulsifier-...

Embodiment 1

[0051] (1) Add 12.3 g of Span-60 and 10 g of n-nonanol into 200 mL of cyclohexane, stir and dissolve at 30° C. and 2000 rpm to obtain a continuous phase.

[0052] (2) Add 10g of 2-acrylamide-2-methylpropanesulfonic acid, 10.6g of N-vinylpyrrolidone, 10g of acrylamide, and 2g of N,N-dimethylacrylamide to 60mL of deionized water , Properly increase the speed to fully dissolve.

[0053] (3) Add 2.1 g of OP-10 and 5.6 g of CaCl to the solution in step (2) 2 , after stirring and dissolving at 800 rev / min, increase the speed appropriately, then slowly add sodium carbonate solution (6.4g sodium carbonate + 22g deionized water) dropwise, and stir at 1000 rev / min at 30°C for 60min.

[0054] (4) Slowly add 6 g of silane coupling agent KH570 dropwise to the solution in step (3), and stir at 60° C. at 1000 rpm for 60 min to obtain a suspension.

[0055] (5) Introduce nitrogen and start stirring, slowly drop the suspension obtained in step (4) into the continuous phase of step (1) (where...

Embodiment 2

[0060] (1) Add 15 g of Span-80 and 10 g of n-octanol to 200 mL of kerosene, stir and dissolve at 25° C. and 1000 rpm to obtain a continuous phase.

[0061] (2) Add 11g of 2-acrylamide-2-methylpropanesulfonic acid, 12.2g of N-vinylpyrrolidone, 11g of acrylamide, and 1.2g of N,N-dimethylpropene into 60mL of deionized water For amides, increase the rotation speed appropriately to fully dissolve them.

[0062] (3) Add 3g of Tween-20 and 6g of CaCl in the solution of step (2) 2 , after stirring and dissolving at 600 rpm, increase the rotation speed appropriately, and then slowly add sodium carbonate solution (5.4g sodium carbonate + 22g deionized water) dropwise, and stir at 1000 rpm at 25°C for 80min.

[0063] (4) 5.6 g of silane coupling agent APTES was slowly added dropwise to the solution in step (3), and stirred at 60° C. at 800 rpm for 60 min to obtain a suspension.

[0064] (5) Introduce nitrogen and start stirring, slowly add the suspension in step (4) dropwise to the con...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
particle sizeaaaaaaaaaa
particle sizeaaaaaaaaaa
particle sizeaaaaaaaaaa
Login to View More

Abstract

The invention relates to the field of oilfield chemistry, and discloses a method for preparing a fluid loss control agent with a core-shell structure. The method comprises the following steps: (1) mixing a solvent, an emulsifier-1 and a co-emulsifier to obtain a continuous phase; ( 2) the aqueous solution containing multiple polymer monomers, emulsifier-2, calcium chloride, sodium carbonate and silane coupling agent are formulated into suspension; (3) the suspension is mixed with the continuous phase to form an emulsion (4) In the presence of an oxidizing agent and a reducing agent, the emulsion is reacted, and the obtained product is subjected to demulsification, filtration, and filter cake washing and drying to obtain the fluid loss control agent. Add 1% w / v of the fluid loss control agent to 4% w / v bentonite base slurry, and the medium pressure fluid loss of the obtained slurry after hot rolling at 220°C for 16 hours is not more than 10.6mL, and the medium pressure fluid loss The reduction rate of the amount relative to the bentonite base slurry is not less than 79.62%, anti-NaCl≥30%, anti-CaCl 2 ≥1%.

Description

technical field [0001] The invention relates to the field of oilfield chemistry, in particular to a fluid loss reducer for water-based drilling fluid with a core-shell structure and excellent performance in high temperature resistance, salt resistance and calcium resistance, a preparation method and application thereof, and a water-based drilling fluid. Background technique [0002] With the increase of formation depth, the formation temperature is getting higher and higher, and during the drilling process, high salinity formations such as saline and gypsum are often encountered. Polymer fluid loss additive molecules mainly interact with clay particles through the functional groups on the side chains to ensure the stability and multi-level dispersion of the drilling fluid, so that the drilling fluid can form dense, low-permeability mud during the drilling process. Cake, reduce the fluid loss of drilling fluid. However, the presence of inorganic salts in drilling fluid will ...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & AuthorityPatents(China)
IPC IPC(8): C08F226/10C08F220/58C08F220/56C08F220/54C08F212/14C08F228/02C09K8/03
CPCC08F226/10C08F212/30C08F220/56C09K8/03C08F220/585C08F220/54C08F228/02
Inventor钟汉毅刘文磊邱正松管颖孔祥政万远周国伟黄维安
OwnerCHINA UNIV OF PETROLEUM (EAST CHINA)