Method for degrading gelled resin
A gelled resin and resin technology, applied in the field of degraded gelled resin, can solve the problems of narrow application range, etc., and achieve the effect of low equipment requirements, simple process, and easy-to-obtain raw materials
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2016-05-18
Abstract
Description
technical field
[0001] The invention belongs to the field of chemical raw materials, and in particular relates to a method for degrading gelled resin. Background technique
[0002] Polyester refers to a polymer oligomer synthesized by polyesterification reaction of polyol and polyacid. According to the saturation of its structure, polyester can be divided into saturated polyester and unsaturated polyester. Unsaturated polyester refers to the polyester with unsaturated double bonds in the main chain, and the polyester without unsaturated double bonds in the main chain is called saturated polyester. Polyester can be widely used as a kind of packaging material. Taking polyester bottle as an example, because the bottle made of this polymer has the advantages of light weight, unbreakable, good odor preservation and good transparency, it has been widely used. Used to pack fruit juice, tea, edible oil, medicine, cosmetics and other items.
[0003] Modification of polyesters with...
Examples
Embodiment 1
[0023] A method for degrading gelatinized resin, comprising the steps of:
[0024] (1) drop into 4.4mol of trimethylolpropane, 0.3 gram of zinc acetate, 1.5 gram of hypophosphorous acid in the reactor, then mix well, heat up to 120°C, and wait for it to completely dissolve;
[0025] (2) the gelled alkyd resin (the vegetable oleic acid that contains 1.04mol, the phthalic anhydride of 2.70mol, the glycerin of 2.27mol in this gelled alkyd resin) is slowly added to the reaction kettle, and with step (1) Mix the solution evenly, then raise the temperature to 240°C, keep it warm, and the reaction time of transesterification degradation is 8 hours. At this time, the kettle liquid is a relatively uniform liquid without obvious lumps or lumps, and the viscosity has no obvious change. Finally, the temperature is lowered to 180°C. ℃;
[0026] (3) Add the vegetable oleic acid of 1.43mol and the phthalic anhydride of 2.84mol in the degradation material that step (2) obtains, be warming up...