Abstract
Description
technical field
[0001] The invention belongs to a coating for processing finished paper. Background technique
[0002] As we all know, cigarette smoke contains a variety of harmful substances. After smoking, the deposition of these harmful ingredients in the human body will cause a variety of diseases in the lungs, respiratory tract, stomach and other organs. Although everyone knows that smoking is harmful to health, cigarettes are refreshing. , A variety of functions to soothe the nerves, proper smoking can make people excited, inspire inspiration, and improve work efficiency, so it is still difficult for smokers to quit smoking.
[0003] Pu-erh tea is a loose tea and pressed tea made from Yunnan big-leaf sun-dried green tea in a certain area of Yunnan Province after post-fermentation. The effect of Pu-erh tea is that the tea is mild in nature, warms the stomach and does not hurt the stomach, which is especially obvious for cooked Pu-erh tea. Second, Pu-erh tea can lowe...
Examples
Embodiment 1
[0021] Add 2kg of pulverized Pu'er ripe tea to 100kg of boiling water, soak for 0.5 hours, filter, take the filtrate, and concentrate the filtrate to a liquid a with a viscosity of 30 seconds measured with a 4 viscosity cup; in another container, first heat 100kg of water To 60 ℃, 12kg carboxymethyl cellulose, 8kg potato starch, 8kg guar gum and water are stirred and mixed to form cross-linked mixed solution b; liquid a and cross-linked mixed solution b are stirred and mixed at a ratio of 1:0.8, A water-based coating for forming paper was prepared.
Embodiment 2
[0023] Add 3kg of crushed Pu'er raw tea to 100kg of boiling water, soak for 1 hour, filter, take the filtrate, and concentrate the filtrate to a liquid a with a viscosity of 31 seconds measured with a 4-viscosity cup; in another container, first heat 100kg of water To 65 ℃, 13kg carboxymethyl cellulose, 9kg potato starch, 12kg guar gum and water are stirred and mixed to form cross-linked mixed solution b; liquid a and cross-linked mixed solution b are stirred and mixed at a ratio of 1:0.9, A water-based coating for forming paper was prepared.
Embodiment 3
[0025] Add 5kg of pulverized Pu'er cooked tea to 100kg of boiling water, soak for 2 hours, filter, take the filtrate, and concentrate the filtrate to a liquid a with a viscosity of 33 seconds measured with a coating 4 viscosity cup; in another container, first heat 100kg of water To 70 ℃, 14kg carboxymethyl cellulose, 10kg potato starch, 12kg guar gum and water are stirred and mixed to form cross-linked mixed solution b; liquid a and cross-linked mixed solution b are stirred and mixed at a ratio of 1:1, A water-based coating for forming paper was prepared.