A kind of marking composition, preparation method and application

A technology for marking and road marking, applied in the field of road materials, can solve problems such as affecting the service life of asphalt pavement, inability to judge the timing of high temperature or low temperature, and hidden dangers of high and low temperature diseases on asphalt pavement, so as to achieve stability and uniformity. Effect

CN108643070BActive Publication Date: 2021-01-26GUANGDONG UNIV OF TECH
10 Cites 0 Cited by

Patent Information

Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Publication Date
2021-01-26

Smart Images

  • Figure 1
    Figure 1
  • Figure 2
    Figure 2
  • Figure 3
    Figure 3
Patent Text Reader

Abstract

The invention belongs to the field of road materials, and in particular relates to a marking composition, a preparation method and an application. A marking composition provided by the invention comprises: an organic reversible heat-sensitive color-changing material, a heat-conducting material, an adhesive, a curing agent, a heat-insulating paint and a road marking paint. A marking composition provided by the present invention, and applying it to high and low temperature early warning marking materials can effectively solve the problem in the prior art that the occurrence of high temperature or low temperature diseases cannot be judged in time, thus causing high and low temperature diseases on asphalt pavement Technical problems that seriously affect the service life of asphalt pavement due to hidden dangers.
Need to check novelty before this filing date? Find Prior Art

Description

technical field

[0001] The invention belongs to the field of road materials, and in particular relates to a marking composition, a preparation method and an application. Background technique

[0002] Asphalt pavement is widely used in the field of expressways in my country because of its good smoothness, driving comfort, safety and road performance. Although asphalt pavement has a good application effect, it is prone to pavement diseases in extreme environments such as high temperature and low temperature.

[0003] Under high temperature conditions, the texture of asphalt materials becomes soft, and severe high-temperature rutting is prone to occur under the action of traffic loads. However, under low-temperature conditions, the texture of asphalt materials becomes brittle and prone to low-temperature cracking, which seriously affects the service life of asphalt pavement. Most of the existing strategies to deal with high and low temperature diseases of asphalt pavement are ...

Examples

Embodiment 1

[0042]The marking composition prepared in this example, in parts by weight, includes 23 parts of heat-sensitive ink, 9 parts of thermally conductive silica gel, 16 parts of water-based acrylic resin, 8 parts of urea-formaldehyde resin, 26 parts of two-component marking paint, silicon carbide 16 parts of ceramic paint, 11 parts of transparent thermal insulation paint, 14 parts of neopentyl glycol diglycidyl ether.

[0043] The preparation method of the marking composition described in this embodiment comprises the following steps:

[0044] (1) Use marking spraying equipment to spray two-component marking paint on the surface of the road surface. After the surface is completely dry, lay thermal silica gel on the surface of the two-component marking paint;

[0045] (2) Apply an appropriate amount of binder water-based acrylic resin on the surface of the heat-conducting silica gel, use heat-sensitive ink to draw high-temperature warning or low-temperature warning words on the road...

Embodiment 2

[0048] The marking composition prepared in this embodiment, in parts by weight, includes 23 parts of heat-sensitive ink, 10 parts of thermally conductive silica gel, 18 parts of water-based acrylic resin, 9 parts of urea-formaldehyde resin, 28 parts of two-component marking paint, silicon carbide 18 parts of ceramic paint, 12 parts of transparent thermal insulation paint, 18 parts of neopentyl glycol diglycidyl ether.

[0049] The preparation method of the marking composition described in this embodiment comprises the following steps:

[0050] (1) Use marking spraying equipment to spray two-component marking paint on the surface of the road surface. After the surface is completely dry, lay thermal silica gel on the surface of the two-component marking paint;

[0051] (2) Apply an appropriate amount of binder water-based acrylic resin on the surface of the heat-conducting silica gel, use heat-sensitive ink to draw high-temperature warning or low-temperature warning words on the...

Embodiment 3

[0054] The marking composition prepared in this embodiment, in parts by weight, includes 24 parts of heat-sensitive ink, 12 parts of thermally conductive silica gel, 20 parts of water-based acrylic resin, 10 parts of urea-formaldehyde resin, 30 parts of two-component marking paint, silicon carbide 20 parts of ceramic paint, 14 parts of transparent thermal insulation paint, 20 parts of neopentyl glycol diglycidyl ether.

[0055] The preparation method of the marking composition described in this embodiment comprises the following steps:

[0056] (1) Use marking spraying equipment to spray two-component marking paint on the surface of the road surface. After the surface is completely dry, lay thermal silica gel on the surface of the two-component marking paint;

[0057] (2) Apply an appropriate amount of binder water-based acrylic resin on the surface of the heat-conducting silica gel, use heat-sensitive ink to draw high-temperature warning or low-temperature warning words on th...