Embodiment 1
[0127] 1. Determination of wood moisture content
[0128] Take random samples from the wood or wood products to be dried, and measure the initial moisture content of the selected wood or wood product samples: weigh the initial weight of the sampled wood (G 0 : 15.5kg), then put the wood in an oven at (100±3)°C to dry to constant weight, and weigh (G 干 : 10kg), wood initial moisture content (M 木初 ,%) is calculated according to the following formula:
[0129] m 木初 =(G 0 -G 干 ) / G 干 ×100%=(15.5-10) / 10×100%=55%
[0130] The size of the test material Daguozi sandalwood in the present embodiment is 2000mm (length) * 40mm (thickness) * 100mm (width).
[0131] 2. Pretreatment of drying medium (adjusting the moisture content of drying medium)
[0132] 2A. Dry the sea sand in the drying medium at a temperature of (100±5)°C, and dry it to a constant weight, that is, until the weight of the drying medium is constant, put the drying medium in a container with a desiccant and cool it...
Embodiment 2
[0169] 1. Determination of wood moisture content
[0170] Except that the size of the red sandalwood is 2000mm (length) * 20mm (thickness) * 100mm (width), the wood initial moisture content is 60%, all the other are identical with embodiment 1;
[0171] 2. Drying medium pretreatment
[0172] Except adding water to the sea sand dried to absolute dryness, and mixing uniformly, adjusting the water content of the drying medium sea sand to 50%, and preparing a pretreatment drying medium with a water content of 50%, the rest are the same as in Example 1 ;
[0173] 3. Palletizing and filling with drying medium
[0174]Except that the loaded pretreatment drying medium is 10cm higher than the top layer of wood in the stack; the distance between two adjacent layers of supports is 6cm (usually 3-18cm), and the top of the wood to be dried on the next layer of support is placed on the same level as the upper layer. Except that the bottoms of the supports are spaced apart by 3.5cm (usual...
Embodiment 3
[0179] 1. Determination of wood moisture content
[0180] Except that the size of the red sandalwood is 2000mm (length) * 20mm (thickness) * 100mm (width), the wood initial moisture content is 30%, all the other are identical with embodiment 1;
[0181] 2. Drying medium pretreatment
[0182] Except adding water to the sea sand dried to absolute dryness, and mixing uniformly, adjusting the water content of the drying medium sea sand to 25%, and preparing a pretreatment drying medium with a water content of 25%, the rest are the same as in Example 1 ;
[0183] 3. Palletizing and filling with drying medium
[0184] Same as embodiment 1;
[0185] 4. Drying treatment of wood / wood products
[0186] Same as Example 1, the drying time is 52h.
[0187] According to the national standard "GB / T 6491-1999 Drying Quality of Sawn Timber", the prepared dry wood was evaluated, and the evaluation results are shown in Table 1.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com