Night vision piece and preparation method thereof
A night vision film, nano technology, applied in the direction of instruments, optics, optical components, etc., can solve the problem of different spectral structures, and achieve the effect of a wide range of applications and good application prospects.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0050] A night vision film suitable for monochromatic green LED backlight and meeting the requirements of night green A (its shape refers to figure 1 ), its preparation method comprises the steps:
[0051] (1) Heat the transparent polycarbonate (PC) masterbatch to 300°C to melt;
[0052] (2) According to the type of LED light source to be matched, according to the transparent masterbatch: the masterbatch doped with nano-linear gold is added to the melted PC masterbatch according to the mass ratio of 1000:3. ;
[0053] (3) AB530 type absorber (belonging to metal complexes) (light with absorption peak 530nm, figure 2 The curve portion of the middle trough) is mixed in the PC master batch that has been doped with gold nanometers to obtain a mixture, and the addition ratio of the AB530 type absorbent is: AB530 type absorbent: PC master batch=1:1000, mass ratio;
[0054] (4) Stir the mixture evenly with a stirrer, then place it in an ultrasonic device with a heating function, a...
Embodiment 2
[0061] A night vision film suitable for monochromatic green LED backlight and meeting the requirements of night green A (its shape refers to figure 1 ), its preparation method comprises the steps:
[0062] (1) Heat the transparent polycarbonate (PC) masterbatch to 300°C to melt;
[0063] (2) According to the type of LED light source to be matched, according to the transparent masterbatch: the masterbatch doped with nano-linear gold is added to the melted PC masterbatch according to the mass ratio of 1000:7. ;
[0064] (3) AB650 type absorber (belonging to phthalocyanines) (light with absorption peak 600-680nm, image 3 The curve portion of the middle trough) is mixed in the PC master batch that has been doped with gold nanometers to obtain a mixture, and the addition ratio of the AB650 type absorbent is: AB650 type absorbent: PC master batch=1.5:10000, mass ratio;
[0065] (4) Stir the mixture evenly with a stirrer, then place it in an ultrasonic device with a heating funct...
Embodiment 3
[0072] A night vision film suitable for monochrome green LED backlight and meeting the requirements of night green B (its shape refers to figure 1 ), its preparation method comprises the steps:
[0073] (1) Heat the transparent polycarbonate (PC) masterbatch to 300°C to melt;
[0074] (2) According to the type of LED light source to be matched, according to the transparent masterbatch: the masterbatch doped with nano-linear gold is added to the melted PC masterbatch according to the mass ratio of 1000:7. ;
[0075] (3) Mix the AB670 type absorber (phthalocyanine) (light absorption peak 670nm, absorb 620nm-680nm light) into the PC masterbatch that has been doped with nano-gold to obtain a mixture, the addition ratio of the AB670 type absorber For: AB670 type absorbent: PC masterbatch = 3:10000, mass ratio;
[0076] (4) Use a stirrer to stir the above-mentioned mixture evenly, then place it in an ultrasonic device with heating function, and carry out ultrasonic vibration on t...
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com