A kind of paint and its construction technology for fair-faced concrete protection
A technology of fair-faced concrete and coatings, applied in the direction of coatings, etc., can solve the problems of concrete lack of decoration, large gaps, rust spots, etc., and achieve the effect of maintaining natural texture and texture and preventing uneven gloss
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0029] A kind of coating that is used for fair-faced concrete protection, its formula is shown in Table 1.
[0030] Table 1
[0031]
[0032] Among the above:
[0033] Wacker E22 silicone polymer emulsion, produced by Wacker;
[0034] Vivid-40 self-crosslinking acrylic acid polymer emulsion, produced by XX company;
[0035] R706, rutile titanium dioxide, produced by DuPont;
[0036] Protectosil SC60 fluorosilicone polymer supplied by Evonik Degussa.
[0037] The preparation method of the product is as follows:
[0038] Add deionized water to the reaction kettle, add Wacker E22 or Protectosil SC60 under the action of stirring, and keep stirring for 30 minutes after the dispersion is uniform, to obtain the primer or top coat in the paint.
[0039] Add deionized water to the reaction kettle, add sodium hexametaphosphate, 2-3168, texanol in turn under stirring, when one component is dispersed or dissolved evenly, the next component can be added, when all components are eve...
Embodiment 2
[0046] With reference to embodiment 1, a kind of coating that is used for fair-faced concrete protection, its formula is shown in Table 2.
[0047] Table 2
[0048]
[0049]
[0050] The preparation method of the product is as follows:
[0051] Add deionized water to the reaction kettle, add Wacker E22 or Protectosil SC60 under the action of stirring, and keep stirring for 30 minutes after the dispersion is uniform, to obtain the primer or top coat in the paint.
[0052] Add deionized water to the reaction kettle, add sodium hexametaphosphate, 2-3168, texanol in turn under stirring, when one component is dispersed or dissolved evenly, the next component can be added, when all components are evenly dispersed , keep stirring at a speed of 750rpm for 5 minutes, after completion, add cement and R706 in turn under the action of stirring, when one component is evenly dispersed, the next component can be added, when all components are evenly dispersed, at a speed of 1000-1500r...
Embodiment 3
[0059] With reference to embodiment 2, a kind of coating that is used for fair-faced concrete protection, its formula is shown in table 3.
[0060] table 3
[0061]
[0062] The preparation method of the product is as follows:
[0063] Add deionized water to the reaction kettle, add Wacker E22 or Protectosil SC60 under the action of stirring, and keep stirring for 30 minutes after the dispersion is uniform, to obtain the primer or top coat in the paint.
[0064]Add deionized water to the reaction kettle, add sodium hexametaphosphate, 2-3168, texanol in turn under stirring, when one component is dispersed or dissolved evenly, the next component can be added, when all components are evenly dispersed , keep stirring at a speed of 750rpm for 5 minutes, after completion, add cement and R706 in turn under the action of stirring, when one component is evenly dispersed, the next component can be added, when all components are evenly dispersed, at a speed of 1000-1500rpm Keep stir...
PUM
Property | Measurement | Unit |
---|---|---|
glass transition temperature | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com