Embodiment 1
[0052] A water-based colorful imitation stone paint, comprising 7% presol solution, color masterbatch and silicone acrylic emulsion, its parts by weight are:
[0053] 10-30 parts of 7% presol solution;
[0054] 30-50 copies of color masterbatch;
[0055] Silicone acrylic emulsion 30-50 parts;
[0056] Described color masterbatch comprises following component, by weight:
[0057] 50-55 parts of deionized water;
[0058] 0.1-0.3 parts of preservatives;
[0059] Dry film antifungal agent 0.2-0.4 parts;
[0060] 0.4-0.8 parts of methyl ethyl hydroxyethyl cellulose;
[0061] Diethanolamine 0.1-0.3 part;
[0062] Dispersant 0.3-0.7 parts;
[0063] Surfactant 0.05-0.2 part;
[0064] 1-5 parts of titanium dioxide;
[0065] Elastic silicone acrylic emulsion 20-40 parts;
[0066] Coalescing aid 0.5-1.5 parts;
[0067] 0.2-0.3 part of defoamer;
[0068] 5-15 parts of 10% lithium magnesium silicate solution;
[0069] Color paste 1-3 parts.
[0070] In addition, the preservat...
Embodiment 2
[0076] The preparation method of water-based colorful imitation stone coating is identical with embodiment 1, and difference is:
[0077] A water-based colorful imitation stone paint, comprising 7% presol solution, color masterbatch and silicone acrylic emulsion, its parts by weight are:
[0078] 20 parts of 7% presol solution;
[0079] 40 parts of color masterbatch;
[0080] Silicone acrylic emulsion 40 parts;
[0081] The parts by weight of the color masterbatch are:
[0082] 52.4 parts of deionized water;
[0083] 0.2 parts of preservatives;
[0084] 0.3 parts of dry film antifungal agent;
[0085] 0.6 parts of methyl ethyl hydroxyethyl cellulose;
[0086] 0.2 part of diethanolamine;
[0087] 0.5 parts of dispersant;
[0088] Surfactant 0.1 part;
[0089] 2.5 parts of titanium dioxide;
[0090] Elastic silicone acrylic emulsion 30 parts;
[0091] 1 part of film-forming aid;
[0092] 0.2 part of defoamer;
[0093] 10 parts of 10% lithium magnesium silicate solutio...
Embodiment 3
[0098] The preparation method of water-based colorful imitation stone coating is identical with embodiment 1, and difference is:
[0099] A water-based colorful imitation stone paint, comprising 7% presol solution, color masterbatch and silicone acrylic emulsion, its parts by weight are:
[0100] 10 parts of 7% presol solution;
[0101] 50 parts of color masterbatch;
[0102] Silicone acrylic emulsion 40 parts;
[0103] Described color masterbatch comprises following component, by weight:
[0104] 55 parts of deionized water;
[0105] 0.1 parts of preservatives;
[0106] 0.2 parts of dry film antifungal agent;
[0107] 0.4 parts of methyl ethyl hydroxyethyl cellulose;
[0108] 0.1 part of diethanolamine;
[0109] Dispersant 0.3 part;
[0110] Surfactant 0.1 part;
[0111] 1 part of titanium dioxide;
[0112] Elastic silicone acrylic emulsion 26.1 parts;
[0113] 0.5 part of film-forming aid;
[0114] 0.2 part of defoamer;
[0115] 15 parts of 10% lithium magnesium...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com