Unlock instant, AI-driven research and patent intelligence for your innovation.

Method for manufacturing base paper for tipping paper suitable for environmental-friendly ink satellite flexo printing technology

A base paper for tipping paper and flexographic printing technology, which is applied in pulp beating method, papermaking, paper, etc., can solve the problems that unit type flexo printing machine cannot meet the requirements, the tension between colors is difficult to control, and the solid density is not enough for printed products, etc. Achieve the effect of good image and text reproduction, excellent color degree, and short printing distance

Active Publication Date: 2021-11-19
MUDANJIANG HENGFENG PAPER CO LTD +1
View PDF7 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] The packaging industry is mostly based on unit-type flexo printing machines, but with the market's requirements for production speed, customers' requirements for printing accuracy, and the country's higher and higher requirements for environmental protection, unit-type flexo printing machines can no longer meet the requirements
The main problem is that the substrate between two adjacent colors is driven by the printing plate, and it is difficult to align the substrate when printing plastic and film with high elasticity and deformation; the tension between colors is not easy to control, once the tension changes If it is too large, the paper and film will break, and the fabric will produce weft arcs. In order to avoid aggravating these problems, the production speed has to be reduced, and the printing efficiency will decrease accordingly.
[0007] Flexographic ink is the only non-toxic ink approved by the American Food and Drug Association among all printing methods. It is mainly made of water-soluble resin, pigment, solvent and related additives through compound grinding. The viscosity is relatively low. If the number of lines is too low, the amount of ink supply is too large, and the edge of the printing plate is easy to accumulate ink, which will cause ghosting on the edge of the printed product; Base paper should have good ink acceptance and certain water penetration resistance

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Method for manufacturing base paper for tipping paper suitable for environmental-friendly ink satellite flexo printing technology
  • Method for manufacturing base paper for tipping paper suitable for environmental-friendly ink satellite flexo printing technology
  • Method for manufacturing base paper for tipping paper suitable for environmental-friendly ink satellite flexo printing technology

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0069] This embodiment is a printing surface coated 5% concentration of oxidized oxide starch (LS-2) and 6kg / ton paper Calen surface sizing agent, non-printing surface coated 5% concentration of oxidized oxide starch (LS-2) and The process of 2kg / ton paper antibody 586 has produced the original paper for the environmental protection ink satellite flexographic printing process. The specific production steps are as follows:

[0070]A method for manufacturing a sheath paper for environmentally-friendly ink satellite flexographic printing technology, including the following steps:

[0071] a, jedding process: two slurrys with bleached long fiber needles, bleaching short fibers 桉 木 两; double disc grinding continuous grouped, bleaching long fiber needle leaf wood pulp is 4.5%, 解 度 度 60 ° SR ~ 66 ° Sr, wet weight 5g ~ 6g; bleaching short fiber eucalyptus pulp is 4.5%, 解 度 64 ° SR ~ 70 ° Sr, bleached long fiber needle leaf plagubed and bleached short fiber eucalyptus According to the ...

Embodiment 2

[0085] In this example, a 6% concentration of oxide starch (LS-2), 3kg / ton paper water repellent 586, 3kg / ton paper water repellent 586, 3kg / ton paper, 5% concentration The oxidized oxide starch (LS-2) and 2 kg / ton of Coral Surface sizing agents have produced a reload paper material that satisfies the environmental ink satellite flexographic printing process, and the specific production steps are as follows:

[0086] a, jedding process: two slurrys with bleached long fiber needles, bleaching short fibers 桉 木 两; double disc grinding continuous grouped, bleaching long fiber needle leaf wood pulp is 4.5%, 解 度 度 60 ° SR ~ 66 ° Sr, wet weight 5g ~ 6g; bleaching short fiber eucalyptus pulp is 4.5%, 解 度 64 ° SR ~ 70 ° Sr, bleached long fiber needle leaf plagubed and bleached short fiber eucalyptus According to the mass ratio of 45% ~ 50%: 50% ~ 55% piring, the upper melt pulp is 66 ° SR ~ 68 ° Sr, and the wet weight is 4.5 g to 5.0 g.

[0087] B, Accessories Add Procedure: Contin...

Embodiment 3

[0093] In this example, a 6% concentration of polyvinyl alcohol (PVA08-99), 6KG / ton, non-printing surface is coated with a 5% concentration of oxidized oxide starch (LS-). 2) Ways of decoction with 2 kg / ton paper Corne sizing agent, producing pick-up paper material that satisfies environmentally-friendly ink satellite flexographic printing processes, and its specific production steps are as follows:

[0094] a, jedding process: two slurrys with bleached long fiber needles, bleaching short fibers 桉 木 两; double disc grinding continuous grouped, bleaching long fiber needle leaf wood pulp is 4.5%, 解 度 度 60 ° SR ~ 66 ° Sr, wet weight 5g ~ 6g; bleaching short fiber eucalyptus pulp is 4.5%, 解 度 64 ° SR ~ 70 ° Sr, bleached long fiber needle leaf plagubed and bleached short fiber eucalyptus According to the mass ratio of 45% ~ 50%: 50% ~ 55% piring, the upper melt pulp is 66 ° SR ~ 68 ° Sr, and the wet weight is 4.5 g to 5.0 g.

[0095] B, Accessories Add Procedure: Continuous 200kg / ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
Cobb valueaaaaaaaaaa
opacityaaaaaaaaaa
Login to View More

Abstract

A method for manufacturing base paper for tipping paper suitable for environmental-friendly ink satellite flexographic printing technology; comprising the following steps: a, beating process: using two kinds of pulp, bleached long-fiber coniferous wood pulp and bleached short-fiber eucalyptus wood pulp; For beating, the beating concentration of bleached long-fiber softwood pulp is 4.5%, the beating degree is 60°SR~66°SR, and the wet weight is 5g~6g; the beating concentration of bleached short-fiber eucalyptus pulp is 4.5%, and the beating degree is 64°SR~ 70°SR, bleached long-fiber coniferous wood pulp and bleached short-fiber eucalyptus pulp, according to the mass ratio of 45% to 50%: 50% to 55% pulping, the pulping degree of the net pulp is 66°SR to 68°SR , Wet weight 4.5g~5.0g; b. Addition process of auxiliary materials: Add 200kg / ton of paper light calcium carbonate, 100kg / ton of paper 325 mesh talcum powder auxiliary materials and 50kg / ton of paper pharmaceutical grade into the prepared mixed pulp Titanium dioxide.

Description

Technical field [0001] The present invention relates to the technical field of tobacco paper sheet, particularly a green ink flexo printing technique is applied tipping base paper manufacturing method. Background technique [0002] Flexographic printing using flexographic plates, the anilox roll aqueous green ink layer applied to a predetermined thickness uniformly in the graphic portion of the printing plate projection, then under the action of the impression cylinder, the graphic portion of the green water-based ink transferred to the surface of the substrate, to form a clear graphic. Divided stacked flexographic printing press, satellite, and three units of formula according to various arrangements. [0003] According to the American Flexographic Technical Association (FTA) to predict the future with the flexible packaging industry needs a substantial increase in flexo print, flexo proportion of share in the packaging sector will grow further. At present, my country's packagin...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): D21H21/16D21D1/02D21G1/00D21H17/28D21H17/36D21H17/52D21H17/56D21H17/67
CPCD21D1/02D21G1/00D21H17/28D21H17/36D21H17/52D21H17/56D21H17/675D21H21/16
Inventor 潘高峰翟继岚都业壮刘玲红邱诗波
Owner MUDANJIANG HENGFENG PAPER CO LTD