Embodiment 1
[0033] (1) Preparation of HATP:
[0034] Dissolve 5 g of attapulgite (ATP) in 100 mL of 0.5M HCl solution and stir in a water bath at 60°C for 2 hours to obtain protonated attapulgite (HATP). Filter and wash the obtained HATP to neutrality, then dry at 70°C, and grind Obtain the HATP of the powder, and set aside.
[0035] (2)CeO 2 Preparation of / HATP composite photocatalyst:
[0036] 0.2523g cerium nitrate hexahydrate Ce(NO3 ) 3 ·6H 2 O and 0.005g HATP were dissolved in 60mL deionized water, stirred to completely dissolve the cerium nitrate, then added 2g NaOH and continued to stir, and the obtained suspension was placed in an autoclave at 160°C for 10h, then taken out and naturally cooled to room temperature , washed with deionized water and ethanol until neutral, and dried at 70°C to obtain CeO 2 / HATP composite photocatalyst.
[0037] (3)In 2 o 3 / CeO 2 Preparation of / HATP composite photocatalyst:
[0038] Weigh 0.0275g hydrated indium nitrate In(NO 3 ) 3 4.5H...
Embodiment 2
[0041] (1) Preparation of HATP:
[0042] Dissolve 5g of attapulgite (ATP) in 100mL of 1.0M HCl solution and stir in a water bath at 60°C for 6h to obtain protonated attapulgite (HATP). Filter and wash the obtained HATP to neutrality, then dry at 70°C, and grind Obtain the HATP of the powder, and set aside.
[0043] (2)CeO 2 Preparation of / HATP composite photocatalyst:
[0044] 0.2523g cerium nitrate hexahydrate Ce(NO 3 ) 3 ·6H 2 O and 0.05g HATP were dissolved in 60mL deionized water, stirred to completely dissolve the cerium nitrate, then added 2g NaOH and continued to stir, and the obtained suspension was placed in an autoclave at 160°C for hydrothermal treatment for 14h, then taken out and naturally cooled to room temperature , washed with deionized water and ethanol until neutral, and dried at 70°C to obtain CeO 2 / HATP composite photocatalyst.
[0045] (3)In 2 o 3 / CeO 2 Preparation of / HATP composite photocatalyst:
[0046] Weigh 0.0825g hydrated indium nitra...
Embodiment 3
[0049] (1) Preparation of HATP:
[0050] Dissolve 5g of attapulgite (ATP) in 100mL of 2.0M HCl solution in a 60°C water bath and stir for 12h to obtain protonated attapulgite (HATP). Filter and wash the obtained HATP to neutrality, then dry at 70°C, and grind Obtain the HATP of the powder, and set aside.
[0051] (2)CeO 2 Preparation of / HATP composite photocatalyst:
[0052] 0.2523g cerium nitrate hexahydrate Ce(NO 3 ) 3 ·6H 2 O and 0.01g HATP were dissolved in 60mL deionized water, stirred to completely dissolve the cerium nitrate, then added 2g NaOH and continued to stir, the obtained suspension was placed in an autoclave for 160°C hydrothermal treatment for 20h, then taken out and naturally cooled to room temperature , washed with deionized water and ethanol until neutral, and dried at 70°C to obtain CeO 2 / HATP composite photocatalyst.
[0053] (3)In 2 o 3 / CeO 2 Preparation of / HATP composite photocatalyst:
[0054] Weigh 0.1375g hydrated indium nitrate In(NO ...