Oxygen-permeable membrane surface coated with modified material and method for preparing composite oxygen-permeable membrane
A technology of composite oxygen-permeable membrane sheet and modified material, which is applied in the field of mixed conductor oxygen-permeable membrane material and its preparation, oxygen-permeable membrane material and its preparation field, and can solve the problem that the oxygen permeability and stability of the mixed-conductor oxygen-permeable membrane are not ideal. and other problems, to achieve the effect of improving oxygen permeability, improving stability, and combining firmness
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2015-10-07
- Estimated Expiration
- Not applicable · inactive patent
Smart Images
Figure 1 Figure 2 Figure 3
Abstract
Description
technical field
[0001] The invention relates to an oxygen-permeable membrane material and a preparation method thereof, in particular to a mixed-conductor oxygen-permeable membrane material used in coke oven gas hydrogen production and a preparation method thereof, which is applied in the technical fields of comprehensive utilization of metallurgical resources and functional ceramics manufacturing . Background technique
[0002] Oxygen-permeable membrane materials have very attractive application prospects in industrial processes that require continuous supply of pure oxygen or oxygen separation, such as partial oxidation of hydrocarbons, oxygen-enriched combustion, and decomposition of carbon dioxide. For example, see image 3 , at a reaction temperature of 750°C, at a helium flow rate of 100 ml min -1 and an air flow rate of 300 ml min -1 Under the condition that BaCo 0.7 Fe 0.21 Nb 0.09 o 3-y (BCFN) The oxygen permeability of a single oxygen permeable membrane is 0...
Examples
Embodiment 1
[0022] In this example, see figure 1 and figure 2 , the method for preparing a composite oxygen-permeable membrane by coating the modified material on the surface of the oxygen-permeable membrane has the following processes and steps:
[0023] 20.434 mmol of Ba(NO 3 ) 2 , 20.434 mmol of Co(NO 3 ) 2 ·6H 2 O, 20.434 mmol of Fe(NO 3 ) 3 9H 2 O and 10.217 mmol of Gd 2 o 3 Dissolve in 100 ml with a concentration of 0.5 mol·L -1 In the aqueous solution of nitric acid, stir until completely dissolved; according to the metal ion: ethylenediaminetetraacetic acid (EDTA): the mass ratio of citric acid is 1: 1: 2, accurately weigh the quality of EDTA and citric acid, add deionized water and Stir to dissolve the organic matter; mix the two obtained solutions, add ammonia water dropwise until the pH of the solution is 6.0, and keep the temperature of the solution at 90°C until the reactant becomes a sol. Dry the obtained sol-like substance at 110°C, take it out after the sol-l...
Embodiment 2
[0027] This embodiment is basically the same as Embodiment 1, especially in that:
[0028] In this embodiment, the method for preparing a composite oxygen-permeable membrane by coating the modified material on the surface of the oxygen-permeable membrane has the following processes and steps:
[0029] 20.434 mmol of Ba(NO 3 ) 2 , 40.868 mmol of Co(NO 3 ) 2 ·6H 2 O and 10.217 mmol of Gd 2 o 3 Dissolve in 100 ml with a concentration of 0.5 mol·L -1 In the aqueous solution of nitric acid, stir until completely dissolved; according to the metal ion: ethylenediaminetetraacetic acid (EDTA): the mass ratio of citric acid is 1:1:2, accurately weigh the quality of EDTA and citric acid, add deionized water and Stir to dissolve the organic matter; mix the two obtained solutions, add ammonia water dropwise until the pH of the solution is 6.5, and keep the temperature of the solution at 95°C until the reactant becomes a sol. Dry the obtained sol-like substance at 105°C, take it out...
Embodiment 3
[0032] This embodiment is basically the same as the previous embodiment, and the special features are:
[0033] In this embodiment, the method for preparing a composite oxygen-permeable membrane by coating the modified material on the surface of the oxygen-permeable membrane has the following processes and steps:
[0034] 20.434 mmol of La(NO 3 ) 3 ·6H 2 O, 20.434 mmol of Co(NO 3 ) 2 ·6H 2 O, 20.434 mmol of Fe(NO 3 ) 3 9H 2 O and 10.217 mmol of Gd 2 o 3 Dissolve in 100 ml of nitric acid aqueous solution with a concentration of 0.5 mol L, stir until completely dissolved; accurately weigh EDTA and To the quality of citric acid, add deionized water and stir to dissolve the organic matter; mix the two obtained solutions, add ammonia water dropwise until the pH of the solution is 6.0, and keep the temperature of the solution at 90°C until the reactant becomes a sol. Dry the obtained sol-like substance at 110°C, take it out after the sol-like substance expands into a spon...
