Slow release material using modified zeolite as carrier, and preparation method and application thereof
A technology of modified zeolite and slow-release materials, which is applied in application, fertilizer mixture, fertilization equipment, etc., can solve the problems of soil compaction and hardening, harmful substances exceeding the standard, aquatic organism death, etc., and achieve long fertilizer effect period, pollution reduction, adsorption Performance and colloid performance enhancing effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] A kind of sustained-release material preparation with modified zeolite as carrier comprises the following steps:
[0023] (1) The natural zeolite is subjected to high temperature treatment at 200°C for 2 hours, crushed and sieved, and soaked in 0.5mol / l hydrochloric acid for 2 hours to dealuminate the skeleton;
[0024] (2) Grinding the zeolite after acid treatment to 200 mesh fine powder with powder equipment after drying;
[0025] (3) According to the mass percentage, 97% of the modified zeolite fine powder is added with 1% of chitosan and 2% of acrylamide and mixed uniformly to prepare an environment-friendly slow-release material.
Embodiment 2
[0027] A kind of sustained-release material preparation with modified zeolite as carrier comprises the following steps:
[0028] (1) The natural zeolite is subjected to high temperature treatment at 250°C for 1.5h, crushed and sieved, and soaked in 1mol / l hydrochloric acid for 1h at the same time to dealuminate the skeleton;
[0029] (2) Grinding the zeolite after acid treatment to 250 mesh fine powder with powder equipment after drying;
[0030] (3) According to the mass percentage, add 2% chitosan and 3% acrylamide to 95% modified zeolite fine powder and mix uniformly to prepare the slow-release material.
Embodiment 3
[0032] A kind of sustained-release material preparation with modified zeolite as carrier comprises the following steps:
[0033] (1) The natural zeolite is subjected to high temperature treatment at 300°C for 3 hours, crushed and sieved, and soaked in 2mol / l hydrochloric acid for 0.5h at the same time to dealuminate the framework;
[0034] (2) Grinding the zeolite after acid treatment to 300 mesh fine powder with powder equipment after drying;
[0035] (3) According to the mass percentage, add 3% chitosan and 1% acrylamide to 96% modified zeolite fine powder and mix uniformly to prepare the slow-release material.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com