Method for preparing phosphorus removal adsorbent by microwave-assisted salting-out method
A microwave-assisted, phosphorus adsorbent technology, applied in chemical instruments and methods, adsorption water/sewage treatment, water/sludge/sewage treatment, etc., can solve the problems of high cost of consumable materials, secondary pollution and phosphorus removal effect, etc. Achieve the effect of cost saving, low cost and strong adsorption effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0032] In this embodiment, a method for preparing a phosphorus-removing adsorbent by microwave-assisted salting-out method, the specific steps are as follows:
[0033] 1) Raw material selection: select well-preserved and undeteriorated eucalyptus leaves as raw materials;
[0034] 2) Slicing: cut the eucalyptus leaf raw material into flakes with scissors;
[0035] 3) Cooking: put the sliced eucalyptus leaves into boiling water and boil for 30 minutes, then clean them for later use; put the cleaned flaky eucalyptus leaves into a large beaker;
[0036] 4) Prepare sodium chloride solution: prepare a sodium chloride solution with a concentration of 0.5mol / L, pour it into a prepared small beaker, pour 50mL, and label it;
[0037] 5) Microwave-assisted solution soaking: put the boiled flaky eucalyptus leaves into a small beaker filled with 0.5mol / L sodium chloride solution, and put the small beaker into a microwave oven for 20 minutes;
[0038] 6) Cleaning: Take out the flaky euc...
Embodiment 2
[0080] A method for preparing a phosphorus-removing adsorbent by using a microwave-assisted salting-out method, the specific steps of which are as follows:
[0081] 1) Raw material selection: select well-preserved and undeteriorated eucalyptus leaves as raw materials;
[0082] 2) Slicing: cut the eucalyptus leaf raw material into flakes with scissors;
[0083] 3) Cooking: put the sliced eucalyptus leaves into boiling water and boil for 20 minutes, then clean them for later use; put the cleaned flaky eucalyptus leaves into a large beaker;
[0084] 4) Prepare sodium chloride solution: prepare a sodium chloride solution with a concentration of 0.6mol / L, pour it into a prepared small beaker, pour 50mL, and label it;
[0085] 5) Microwave-assisted solution soaking: put the boiled flaky eucalyptus leaves into a small beaker filled with 0.6mol / L sodium chloride solution, and put the small beaker into a microwave oven for 15 minutes;
[0086] 6) Cleaning: Take out the flaky eucaly...
Embodiment 3
[0093] A method for preparing a phosphorus-removing adsorbent by using a microwave-assisted salting-out method, the specific steps of which are as follows:
[0094] 1) Raw material selection: select well-preserved and undeteriorated eucalyptus leaves as raw materials;
[0095] 2) Slicing: cut the eucalyptus leaf raw material into flakes with scissors;
[0096] 3) Cooking: put the sliced eucalyptus leaves into boiling water and boil for 25 minutes, then clean them for later use; put the cleaned flaky eucalyptus leaves into a large beaker;
[0097] 4) Prepare sodium chloride solution: prepare a sodium chloride solution with a concentration of 0.3mol / L, pour it into a prepared small beaker, pour 50mL, and label it;
[0098] 5) Microwave-assisted solution soaking: put the boiled flaky eucalyptus leaves into a small beaker filled with sodium chloride solution, and put the small beaker into a microwave oven for 30 minutes;
[0099] 6) Cleaning: Take out the flaky eucalyptus leav...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com