A technology for railway freight cars and bogies, which is applied in the field of component vibration damping materials, can solve the problems of poor physical and mechanical properties, poor elastic recovery ability, and large heat generation of rubber, and achieves improved mechanical and physical properties, improved elastic recovery ability, and reduced crystallization. sexual effect
Patent Information
- Authority / Receiving Office
- CN · China
- Current Assignee / Owner
- Publication Date
- 2010-12-22
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention relates to a component vibration damping material of a railway freight car, in particular to an elastic side support body material of a railway freight car bogie used for manufacturing the elastic side support body of a railway freight car. Background technique
[0002] The elastic side bearing is the key rubber part of the bogie. The elastic side bearing is installed in the side bearing box of the bolster to support the car body, play a supporting and buffering role, improve the rotation constraint between the bogie and the car body and the roll restraint of the car body, and restrain the bogie shaking head and the car body roll The main snake is unstable. Existing rubber materials used to manufacture elastic side bearings have poor physical and mechanical properties, poor elastic recovery ability at low temperature, poor fatigue resistance with metal composite products, and large heat generation of rubber under motion. defect. Conte...
Examples
Embodiment 1
[0007] Embodiment 1: 80 parts of natural rubber, 25 parts of butadiene rubber, 6 parts of zinc oxide, 0.8 part of stearic acid, 1.5 parts of anti-aging agent 4010NA, 1 part of anti-aging agent D, 1 part of microcrystalline paraffin, 1 part of dispersant D-4A 1 part, 1 part of accelerator CZ, 1.5 parts of sulfur, 0.5 part of accelerator TMTD (industrial grade), 25 parts of Zhongchao wear-resistant carbon black, 20 parts of fast extruded carbon black, 6 parts of low-temperature plasticizer.
Embodiment 2
[0008] Example 2: 100 parts of natural rubber, 10 parts of butadiene rubber, 4 parts of zinc oxide, 1.2 parts of stearic acid, 1 part of anti-aging agent 4010NA, 2 parts of anti-aging agent D (industrial grade), 0.8 part of microcrystalline paraffin, dispersant D 2 parts of -4A, 1.5 parts of accelerator CZ, 1.2 parts of sulfur, 0.8 parts of accelerator TMTD, 40 parts of Zhongchao wear-resistant carbon black, 10 parts of fast extruded carbon black, and 8 parts of low-temperature plasticizer.
[0009] The manufacturing process of above-mentioned embodiment is as follows:
[0010] 1. Equipment: Two-roller open mill XK-160, XN-35L internal mixer, rubber filter 250, electronic scale (maximum weighing 100Kg, sensing capacity 5g), electronic platform scale (maximum weighing 10Kg, sensing capacity Amount 1g), electronic balance (maximum weighing 500g, sensitivity 0.01g).
[0011] 2. Tools: tools such as trays, scribing knives, and charging boxes.
[0012] 3. Weighing: Weigh each com...