A technology of formaldehyde scavenger and mineral crystal, which is applied in deodorization, separation of dispersed particles, chemical instruments and methods, etc., can solve the problems of secondary pollution of products, unsatisfactory formaldehyde removal effect, etc., and achieve strong air purification effect, strong formaldehyde The effect of scavenging
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] Embodiment 1: the preparation of mineral crystal formaldehyde scavenger for decoration
[0017] Pulverize attapulgite, bentonite, sepiolite, diatomaceous earth, zeolite, zirconium phosphate and nano titanium dioxide.
[0018] Weigh:
[0019] Attapulgite 10 kg, bentonite 15 kg, sepiolite 10 kg, diatomite 4 kg, zeolite 10 kg, zirconium phosphate 15 kg and nano titanium dioxide 10 kg.
[0020] The attapulgite, bentonite, sepiolite, diatomaceous earth, zeolite, zirconium phosphate and nano-titanium dioxide are uniformly mixed to obtain the mineral crystal formaldehyde scavenger for decoration of the present invention. Take 50 grams and pack into a breathable non-woven bag for subsequent use.
[0021] A newly renovated hotel room in Shanghai with a usable area of 20m 2 , the concentration of formaldehyde is 0.61mg / m 3 A total of 10 packs (100 grams per pack) of mineral crystal formaldehyde scavenger for decoration in this embodiment were placed in multiple places in th...
Embodiment 2
[0022] Embodiment 2: the preparation of mineral crystal formaldehyde scavenger for decoration
[0023] Pulverize attapulgite, bentonite, sepiolite, diatomaceous earth, zeolite, zirconium phosphate and nano titanium dioxide.
[0024] Weigh:
[0025] 12 kg of attapulgite, 12 kg of bentonite, 12 kg of sepiolite, 3 kg of diatomaceous earth, 12 kg of zeolite, 12 kg of zirconium phosphate and 12 kg of nano-titanium dioxide.
[0026] The attapulgite, bentonite, sepiolite, diatomaceous earth, zeolite, zirconium phosphate and nano-titanium dioxide are uniformly mixed to obtain the mineral crystal formaldehyde scavenger for decoration of the present invention. Take 50 grams and pack into a breathable non-woven bag for subsequent use.
[0027] A newly renovated hotel room in Shanghai with a usable area of 20m 2 , the concentration of formaldehyde is 0.74mg / m 3 A total of 10 packs (100 grams per pack) of mineral crystal formaldehyde scavenger for decoration in this embodiment were p...
Embodiment 3
[0028] Embodiment 3: the preparation of mineral crystal formaldehyde scavenger for decoration
[0029] Pulverize attapulgite, bentonite, sepiolite, diatomaceous earth, zeolite, zirconium phosphate and nano titanium dioxide.
[0030] Weigh:
[0031] 15 kg of attapulgite, 10 kg of bentonite, 15 kg of sepiolite, 2 kg of diatomite, 15 kg of zeolite, 10 kg of zirconium phosphate and 15 kg of nano-titanium dioxide.
[0032] The attapulgite, bentonite, sepiolite, diatomaceous earth, zeolite, zirconium phosphate and nano-titanium dioxide are uniformly mixed to obtain the mineral crystal formaldehyde scavenger for decoration of the present invention. Take 50 grams and pack into a breathable non-woven bag for subsequent use.
[0033] A newly renovated hotel room in Shanghai with a usable area of 20m 2 , the concentration of formaldehyde is 0.69mg / m 3 A total of 10 packs (100 grams per pack) of the mineral crystal formaldehyde scavenger for decoration of this embodiment were placed...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com