Composite fire-retardant glass laminating solution, preparation method thereof and composite fire-retardant glass
A technology of fireproof glass and potassium water glass, applied in the field of safety glass, can solve the problems of difficult control of flow direction, generation of bubbles in lamination liquid, insufficient hardness of fireproof layer, etc., and achieve the effect of eliminating bubbles and avoiding corrosion.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] (1) Weigh the raw materials of composite fireproof glass laminating liquid according to the following weight: (kg)
[0028] 25 potassium silicate with a modulus of 3.3-3.4, 100 deionized water, 0.5 sucrose, 0.25 potassium dihydrogen phosphate, 0.02 defoamer BYK-024, 0.15 leveling agent RH-212, 0.1 sodium fluorosilicate.
[0029] (2) Preparation of composite fireproof glass lamination liquid, including the following steps:
[0030] Add 25 kg of potassium water glass with a modulus of 3.3-3.4 into a container containing 100 kg of deionized water, and stir for 2 hours to disperse the potassium water glass evenly to form a potassium water glass base solution;
[0031] Add 0.5kg sucrose in the basic solution, continue to stir;
[0032] After stirring evenly, add 0.25kg potassium dihydrogen phosphate and continue stirring;
[0033] After stirring evenly, add 0.02kg of defoamer BYK-024, and stir at a high speed of 5000-6000r / min for 30 minutes to disperse the defoamer evenly...
Embodiment 2
[0045] (1) Weigh the raw materials of composite fireproof glass laminating liquid according to the following weight: (kg)
[0046] 50 modulus is 3.3-3.4 potassium water glass, 100 deionized water, 0.5 sucrose, 0.25 potassium dihydrogen phosphate, 0.02 defoamer BYK-024, 0.15 leveling agent RH-212, 0.1 sodium fluorosilicate.
[0047] (2) Preparation of composite fireproof glass lamination liquid:
[0048] The preparation method is the same as in Example 1.
[0049] (3) Prepare composite fire-resistant glass with the lamination solution provided in this example:
[0050] The preparation method is the same as in Example 1.
Embodiment 3
[0052] (1) Weigh the raw materials of composite fireproof glass laminating liquid according to the following weight: (kg)
[0053] 75 modulus is 3.3-3.4 potassium water glass, 100 deionized water, 0.5 sucrose, 0.25 potassium dihydrogen phosphate, 0.02 defoamer BYK-024, 0.15 leveling agent RH-212, 0.1 sodium fluorosilicate.
[0054] (2) Preparation of composite fireproof glass lamination liquid:
[0055] The preparation method is the same as in Example 1.
[0056] (3) Prepare composite fire-resistant glass with the lamination solution provided in this example:
[0057] The preparation method is the same as in Example 1.
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
modulus | aaaaa | aaaaa |
refractive index | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com