Method used for purifying sodium tungstate solution

A sodium tungstate solution technology, applied in the field of metallurgy, can solve the problems of excessive ammonium paratungstate cation elements, affecting tungsten adsorption capacity, poor comprehensive impurity removal effect, etc., and achieve the effect of reducing production costs

Inactive Publication Date: 2015-10-14
CHONGYI ZHANGYUAN TUNGSTEN
View PDF7 Cites 13 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

This method may have poor comprehensive impurity removal effect, or may introduce a large amount of anions (such as chloride ions, sulfate ions, nitrate ions, etc.), which will seriously affect the adsorption capacity of tungsten in the subsequent ion exchange process. Impurity cations can easily cause ammonium paratungstate cation elements to exceed the standard
[0005] Therefore, in the hydrometallurgical process of tungsten, the method of purifying the sodium tungstate liquid with high impurity content needs to be improved

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Method used for purifying sodium tungstate solution
  • Method used for purifying sodium tungstate solution
  • Method used for purifying sodium tungstate solution

Examples

Experimental program
Comparison scheme
Effect test

specific Embodiment

[0037] According to a specific embodiment of the present invention, the method includes the following steps: adding waste tungsten oxide, waste ammonium paratungstate, tungstic acid and waste cemented carbide into the sodium tungstate solution at 50-100° C. at least one of the sodium tungstate solution, and keep stirring to adjust the pH value of the sodium tungstate solution to 8.0-10.0, so as to precipitate silicon to obtain the first sodium tungstate mixed solution containing the silicon precipitation; to the first sodium tungstate solution; adding magnesium salt to the sodium tungstate mixed solution to obtain the second sodium tungstate mixed solution; heating the second sodium tungstate mixed solution to a temperature of not lower than 50°C, and continuously stirring the second sodium tungstate mixed solution , and keep the temperature for 1-3 hours, so as to obtain the third sodium tungstate mixed solution containing the precipitate; and filter the third sodium tungstate...

Embodiment 1

[0042] For containing WO 3 232.7g / L, F 748ppm, P 0.120g / L, SiO 2 The method that 220ppm of sodium tungstate feed liquid is purified is as follows:

[0043] 1. Take 200ml of sodium tungstate feed solution, heat it to about 80°C, and add tungstic acid under stirring conditions. When pH=8~9, stop feeding.

[0044] 2. Add 2.4 g of analytically pure basic magnesium carbonate powder, stir continuously, and keep the temperature for 3 hours to obtain a mixed solution containing precipitates.

[0045] 3. Filter the mixed solution obtained in the previous step to obtain filtrate and residue.

[0046] 4. Determine the composition of the filtrate and slag, as follows:

[0047] Filtrate composition

[0048]

[0049] Composition of slag

[0050]

[0051] It can be found from the above table that the sodium tungstate feed liquid obtained by the purification process of the method of the present invention contains impurity elements F, P, As and SiO. 2 After sufficient precipitation...

Embodiment 2

[0053] For containing WO 3 232.7g / L, F 748ppm, P 0.120g / L, SiO 2 The method that 220ppm of sodium tungstate feed liquid is purified is as follows:

[0054] 1. Take 200ml of sodium tungstate feed solution, heat it to about 80°C, and add tungsten oxide under stirring conditions. When pH=8~9, stop feeding.

[0055] 2. Add 2g of magnesium oxide, keep stirring for 3h, to obtain a mixed solution containing precipitation

[0056] 3. Filter the mixed solution obtained in the previous step to obtain filtrate and residue.

[0057] 4. Determine the composition of the filtrate and slag, as follows:

[0058] Filtrate composition

[0059]

[0060] Composition of slag

[0061]

[0062] From the above table, it can be found that the sodium tungstate feed liquid obtained through the purification treatment of the method of the present invention, the impurity elements F, P, As and Si are fully precipitated, the content of the above-mentioned impurity elements in the filtrate is signif...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention discloses a method used for purifying a sodium tungstate solution. The method comprises following steps: at 50 to 100 DEG C, pH value of the sodium tungstate solution is adjusted so as to realize silicon precipitation and obtain a first sodium tungstate mixed solution containing silicon precipitates; a magnesium salt is added into the first sodium tungstate mixed solution so as to obtain a second sodium tungstate mixed solution; at a temperature of 50 DEG C or higher, stirring is carried out continuously so as to obtain a third sodium tungstate mixed solution containing precipitates; and the third sodium tungstate mixed solution is subjected to filtration so as to obtain a filtrate, wherein the filtrate is the purified sodium tungstate solution. According to the method, solid salts are adopted for purification and processing, so that comprehensive removing of fluorine, phosphorus, arsenic, and silicon can be realized, and influences on tungstate ion exchange and product purity caused by introducing of impurity negative ions and positive ions are avoided. After treatment, content of impurities, such as fluorine, phosphorus, arsenic, and silicon, in the sodium tungstate solution is reduced greatly.

Description

technical field [0001] The invention relates to the field of metallurgy, in particular to a method for purifying sodium tungstate solution. Background technique [0002] Tungsten concentrates are usually treated with acid or alkali. At present, domestic tungsten smelting enterprises mainly use NaOH decomposition process. During the decomposition process, impurities such as phosphorus, arsenic, silicon, tin, fluorine and other impurities in the raw materials will be decomposed and enter the sodium tungstate feed solution. For example, when a factory in my country conducts high-pressure leaching of wolframite concentrate at 135°C, the leaching rates of phosphorus, arsenic and silicon in the raw materials are 30%-40%, 35%-42% and 20%-25%, respectively. Up to 1g / L, in addition to other impurities such as tin. It can be seen that the sodium tungstate feed solution obtained by decomposition contains a large amount of impurities. These impurity components will hinder the treatmen...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C01G41/00
Inventor 邓声华龚丹丹黄泽辉李红超邓登飞
Owner CHONGYI ZHANGYUAN TUNGSTEN
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products