A kind of water-based coating for wine bottle and preparation method thereof
A water-based coating and water-based technology, applied in polyester coatings, epoxy resin coatings, coatings, etc., can solve problems such as environmental pollution, achieve low glass transition temperature, facilitate large-scale industrial production, and simple steps.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0032] A kind of water-based coating that is used for wine bottle surface coating, the preparation method of this water-based coating, the steps are as follows:
[0033] 1) Add 40 parts of water-based epoxy acrylic resin of model WA-360E to the container by weight, then stir with a high-speed disperser, gradually add 0.1 part of ammonia neutralizer dropwise while stirring, and the stirring speed is 500r / min, After stirring for 4 minutes, test that the pH value of the mixed liquid is 8.0, stop stirring, and proceed to the next step;
[0034] 2) Add 10 parts of INEOS-R717 partially methylated amino resin curing agent, 0.3 parts of TEGO-270 wetting agent, 0.3 parts of EFKA-3772 leveling agent, 0.1 parts into the container in sequence 1 part of antifoaming agent of BYK-028 model, 0.1 part of antifoaming agent of Surfynol 104E, and then stir with a high-speed disperser at a stirring speed of 500r / min, and disperse for 5 minutes;
[0035] 3) Add 20 parts of water-based red paste an...
Embodiment 2
[0041] A kind of water-based coating that is used for wine bottle surface coating, the preparation method of this water-based coating, the steps are as follows:
[0042] 1) Add 42 parts of water-based epoxy acrylic resin to the container by weight, then stir with a high-speed disperser, gradually add 0.15 parts of ammonia neutralizer dropwise while stirring, the stirring speed is 700r / min, after 5min, test the mixed liquid When the pH value is 8.4, stop stirring and proceed to the next step;
[0043] 2) Add 10.6 parts of INEOS-R717 partially methylated amino resin curing agent, 0.35 parts of TEGO-270 wetting agent, 0.4 parts of EFKA-3772 leveling agent, 0.2 parts into the container in sequence One part model is BYK-028 defoamer, 0.15 part model is Surfynol 104E antifoam agent, then stir with high-speed disperser, stirring speed is 700r / min, disperse for 7 minutes;
[0044] 3) Add 22 parts of water-based red paste and 2 parts of coupling agent to the container, and finally add...
Embodiment 3
[0050] A kind of water-based coating that is used for wine bottle surface coating, the preparation method of this water-based coating, the steps are as follows:
[0051] 1) Add 45 parts of water-based epoxy acrylic resin to the container by weight, then stir with a high-speed disperser, gradually add 0.2 parts of ammonia neutralizer dropwise while stirring, the stirring speed is 800r / min, after 6min, test the mixed liquid When the pH value is 8.5, stop stirring and proceed to the next step;
[0052] 2) Add 11 parts of INEOS-R717 partially methylated amino resin curing agent, 0.4 parts of TEGO-270 wetting agent, 0.5 parts of EFKA-3772 leveling agent, 0.3 parts into the container One part model is defoamer BYK-028, 0.2 part model is antifoam agent Surfynol 104E, then stir with high-speed disperser, stirring speed is 800r / min, disperse for 10 minutes;
[0053] 3) Add 25 parts of water-based red paste and 3 parts of coupling agent to the container, and finally add 16 parts of deion...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com