A kind of preparation method of preparing chrome tanning agent with carboxymethyl cellulose
A technology of carboxymethyl cellulose and chrome tanning agent, applied in the field of leather chemical industry, can solve the problems of low absorption rate of chrome tanning agent, limited storage, high use cost, etc., achieve excellent tanning performance, reduce use cost, and good comprehensive performance Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] (1) Weigh 40 parts of carboxymethyl cellulose and swell with 400 parts of water for 2 hours;
[0021] (2) Dissolve 100 parts of potassium dichromate with a mass concentration of 100% in water with a mass of 400 parts to obtain a potassium dichromate solution, and then pour it into an acid-resistant Add (133.3-B) concentrated sulfuric acid with a mass concentration of 100% into the container;
[0022] (3) Slowly add carboxymethyl cellulose swollen with water into the reaction vessel containing potassium dichromate solution and concentrated sulfuric acid solution under stirring, and keep the reaction temperature at 95°C until the reaction is completed, and the solution is blue-green; check The color and alkalinity of the tanning liquor, and adjust the reaction solution; if the color of the tanning liquor is slightly yellowish, carboxymethyl cellulose needs to be added to continue the reaction until there is no yellowish shadow; if the alkalinity is slightly lower, soda as...
Embodiment 2
[0026] (1) Weigh 30 parts of carboxymethyl cellulose and swell with 300 parts of water for 3 hours;
[0027] (2) Dissolve 100 parts of potassium dichromate with a mass concentration of 100% in 500 parts of water to obtain a potassium dichromate solution, and then pour it into an acid-resistant Add (133.3-B) concentrated sulfuric acid with a mass concentration of 100% into the container;
[0028] (3) Slowly add carboxymethyl cellulose swollen with water into the reaction vessel containing potassium dichromate solution and concentrated sulfuric acid solution under stirring, and keep the reaction temperature at 95°C until the reaction is completed, and the solution is blue-green; check The color and alkalinity of the tanning liquor, and adjust the reaction solution; if the color of the tanning liquor is slightly yellowish, carboxymethyl cellulose needs to be added to continue the reaction until there is no yellowish shadow; if the alkalinity is slightly lower, soda ash needs to b...
Embodiment 3
[0032] (1) Weigh 50 parts of carboxymethyl cellulose and swell with 450 parts of water for 5 hours;
[0033] (2) Dissolve 100 parts of potassium dichromate with a mass concentration of 100% in water with a mass of 400 parts to obtain a potassium dichromate solution, and then pour it into an acid-resistant Add (133.3-B) concentrated sulfuric acid with a mass concentration of 100% into the container;
[0034] (3) Slowly add carboxymethyl cellulose swollen with water into the reaction vessel containing potassium dichromate solution and concentrated sulfuric acid solution under stirring, and keep the reaction temperature at 95°C until the reaction is completed, and the solution is blue-green; check The color and alkalinity of the tanning liquor, and adjust the reaction solution; if the color of the tanning liquor is slightly yellowish, carboxymethyl cellulose needs to be added to continue the reaction until there is no yellowish shadow; if the alkalinity is slightly lower, soda as...
PUM