Leather finishing agent capable of enhancing mechanical properties and ultraviolet resistance of leather and preparation method of leather finishing agent
A technology of leather finishing agent and mechanical properties, which is applied in small raw hide/large raw hide/leather/fur treatment, small raw hide/large raw hide/leather hide/fur chemical treatment, leather surface treatment, etc., which can solve the problem of long preparation time of finishing agent , leather single performance improvement, complex preparation process and other problems, to achieve the effect of green preparation method, low production cost, high preparation reaction efficiency
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0031] A preparation method of a leather finishing agent capable of enhancing leather mechanical properties and UV resistance, comprising the following steps:
[0032] (1) add reaction raw material gallic acid 1kg in reactor, add the acetic acid of 5kg, obtain gallic acid acid liquid;
[0033] (2) Add 1 part of reaction auxiliary hexamethylenetetramine to the gallic acid solution, raise the reaction temperature to 100° C., and react for 0.5 hours to obtain the reaction solution;
[0034] (3) After reducing the temperature of the reaction solution to 50° C., add 10 kg of distilled water and hydrolyze for 0.5 hour to obtain the leather finishing agent.
[0035] The leather finishing agent is used as the finishing process of tanned leather (taking condensed tanning agent vegetable tanned leather as an example), and the properties of the leather after finishing are characterized. Take a 10mm wide and 50mm leather test sample after finishing, and use a multifunctional tensile mach...
Embodiment 2
[0038] A preparation method of a leather finishing agent capable of enhancing leather mechanical properties and UV resistance, comprising the following steps:
[0039] (1) Add 1 kg of reaction raw material catechin in the reactor, add the trifluoroacetic acid of 8 kg, obtain catechin acid liquid;
[0040] (2) Add 2 kg of reaction auxiliary hexamethylenetetramine to the catechin acid solution, raise the reaction temperature to 90° C., and react for 1.5 hours to obtain the reaction solution;
[0041] (3) After reducing the temperature of the reaction solution to 40° C., add 12 kg of distilled water and hydrolyze for 0.5 hour to obtain the leather finishing agent.
[0042] The leather finishing agent is used in the finishing process of tanned leather (taking chrome tanned leather as an example), and the properties of the leather after tanning are characterized. Take a 10mm wide and 50mm leather test sample after finishing, and use a multifunctional tensile machine to measure its...
Embodiment 3
[0045] A preparation method of a leather finishing agent capable of enhancing leather mechanical properties and UV resistance, comprising the following steps:
[0046] (1) add reaction raw material tannic acid 1kg in reactor, add the polyphosphoric acid of 10kg, obtain tannic acid acid liquid;
[0047] (2) Add 3 kg of reaction aid hexamethylenetetramine to the tannic acid solution, raise the reaction temperature to 80° C., and react for 2 hours to obtain the reaction solution;
[0048] (3) After reducing the temperature of the reaction solution to 30° C., add 20 kg of distilled water and hydrolyze for 1 hour to obtain the leather finishing agent.
[0049] The leather finishing agent is used as the finishing process of tanned leather (take hydrolyzed tanning agent vegetable tanned leather as an example), and the properties of the leather after finishing are characterized. Take a 10mm wide and 50mm leather test sample after finishing, and use a multifunctional tensile machine t...