Natural-degradation environment-friendly flowerpot and manufacture method thereof
A production method and technology for flower pots, which are applied in the fields of botanical equipment and methods, container cultivation, gardening, etc., can solve the problems of difficulty in adapting to flower growth, expensive wooden flower pots, fragile ceramic flower pots, etc. Cracking ability, soft color, brittleness reduction effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] A naturally degradable environment-friendly flower pot and a manufacturing method thereof, comprising the following steps:
[0022] ① After crushing rice husk, bamboo powder and soybean powder, pass through a 60-100 mesh sieve to obtain the sieve material;
[0023] ②Take 25g of sifted rice powder, 12g of bamboo powder, 13g of soybean powder, and 2g of pigment, mix them into 50g of plant fiber powder, take 32g of modified amino resin, 7g of isocyanate, and 11g of oxidized starch, mix them into 50g of adhesive, and mix 50g of plant fiber powder and 50g of adhesive are put into a mixer and stirred to obtain a mixture;
[0024] ③ Add 1g of mold release agent—oxidized polyethylene wax (OPE) to the mixture, and stir fully to obtain a mixed molding material;
[0025] ④Take the molding mixture out of the mixer, dehydrate it at 70°C, and control the moisture content to ≤15%, to obtain the molding mixture;
[0026] ⑤Put the above-mentioned molding material into the mold, the te...
Embodiment 2
[0029] A naturally degradable environment-friendly flower pot and a manufacturing method thereof, comprising the following steps:
[0030] ① After crushing rice husk, bamboo powder and soybean powder, pass through a 60-100 mesh sieve to obtain the sieve material;
[0031] ②Take 35g of sifted rice powder, 8g of bamboo powder, 15g of soybean powder, and 2g of pigment, and mix them into 60g of plant fiber powder; take 24g of modified amino resin, 8g of isocyanate, and 8g of oxidized starch, and mix them into 40g of adhesive; mix 60g of plant fiber and 40g of adhesive is put into a mixer and stirred to obtain a mixture;
[0032] ③ Add 2g of mold release agent—oxidized polyethylene wax (OPE) to the mixture, and stir thoroughly to obtain a mixed molding material;
[0033] ④Take out the molding compound from the mixer, dehydrate it at 85°C, control the moisture content to ≤15%, and obtain the molding compound;
[0034] ⑤Put the above-mentioned molding material into the mold, the te...
Embodiment 3
[0037] A naturally degradable environment-friendly flower pot and a manufacturing method thereof, comprising the following steps:
[0038] ① After crushing rice husk, bamboo powder and soybean powder, pass through a 60-100 mesh sieve to obtain the sieve material;
[0039] ②Take 32g of sifted rice powder, 18g of bamboo powder, and 15g of soybean powder, mix them into 65g of plant fiber powder, take 18g of modified amino resin, 10g of isocyanate, and 7g of oxidized starch, mix them into 35g of adhesive, put 65g of plant fiber and 35g of adhesive into Stir in a mixer to obtain a mixture;
[0040] ③ Add 1.5g of mold release agent—oxidized polyethylene wax (OPE) to the mixture, and stir thoroughly to obtain a mixed molding material;
[0041] ④Take out the molding compound from the mixer, dehydrate it at 80°C, and control the moisture content to ≤15%, to obtain the molding compound;
[0042] ⑤Put the above-mentioned molding material into the mold, the temperature is 130-160°C, the...