A kind of rosin sizing agent and preparation method thereof

A technology of sizing agent and rosin glue, which is applied in the direction of rosin addition, water repellent addition, non-fiber pulp addition, etc. It can solve the problems of corrosivity, dirt generation, foam, and poor oil resistance in papermaking equipment, and achieve softening The effect of point height, improved water resistance, and enhanced hydrophobic binding force

Active Publication Date: 2022-04-22
浙江百斯特化工有限公司
View PDF0 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] In the existing technology, in the sizing process, in order to increase the adhesion effect of the sizing agent to the paper, aluminum sulfate is often added, but the addition of aluminum sulfate is easy to cause corrosion to the papermaking equipment, resulting in dirt, foam and other effects. The domestic paper industry is A lot of work has been done to achieve neutral and alkaline sizing, and a lot of progress has been made in the development of sizing agents, but there are still poor sizing properties, such as low adhesion rate, poor stability, and water resistance. , poor oil resistance and other issues

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0037] A kind of rosin sizing agent and preparation method thereof, its raw material formula comprises the component of parts by weight:

[0038] 30 parts of cationic rosin gum; 10 parts of reinforced rosin gum; 10 parts of modified talc; 15 parts of cyclodextrin; 15 parts of cetyltrimethylammonium chloride; 5 parts of polyglycerol alkyl ether; Parts; 4 parts of 3-aminopropyltrimethoxysilane.

[0039] Concrete preparation method is as follows:

[0040] A1, the cationic rosin is heated and melted, then added to the cyclodextrin aqueous solution, and stirred for 20 minutes;

[0041] A2, add chitosan, stir for 10 minutes, the temperature is 50 ℃;

[0042] A3. Add modified talcum powder, cetyltrimethylammonium chloride and polyglycerol alkyl ether, stir for 10 minutes at a temperature of 50°C, stir until no precipitation occurs, and obtain a rosin sizing agent;

[0043] A4. Heat and melt the strengthened rosin gum, and add trimethylolpropane in batches, with an interval of 20 m...

Embodiment 2

[0048] A kind of rosin sizing agent and preparation method thereof, its raw material formula comprises the component of parts by weight:

[0049] 35 parts of cationic rosin gum; 12 parts of reinforced rosin gum; 15 parts of modified talc; 18 parts of cyclodextrin; 12 parts of cetyltrimethylammonium chloride; 4 parts of polyglycerol alkyl ether; Parts; 5 parts of 3-aminopropyltrimethoxysilane.

[0050] Concrete preparation method is as follows:

[0051] A1, the cationic rosin is heated and melted, then added to the cyclodextrin aqueous solution, and stirred for 20 minutes;

[0052] A2, add chitosan, stir for 10 minutes, the temperature is 50 ℃;

[0053] A3. Add modified talcum powder, cetyltrimethylammonium chloride and polyglycerol alkyl ether, stir for 10 minutes at a temperature of 70°C, stir until no precipitation occurs, and obtain a rosin sizing agent;

[0054] A4. Heat and melt the strengthened rosin gum, and add trimethylolpropane in batches, with an interval of 25 min...

Embodiment 3

[0059] A kind of rosin sizing agent and preparation method thereof, its raw material formula comprises the component of parts by weight:

[0060] 40 parts of cationic rosin gum; 12 parts of reinforced rosin gum; 15 parts of modified talcum powder; 20 parts of cyclodextrin; 18 parts of cetyltrimethylammonium chloride; 6 parts of polyglycerol alkyl ether; Parts; 5 parts of 3-aminopropyltrimethoxysilane.

[0061] Concrete preparation method is as follows:

[0062] A1, the cationic rosin is heated and melted, then added to the cyclodextrin aqueous solution, and stirred for 20 minutes;

[0063] A2, add chitosan, stir for 10 minutes, the temperature is 50 ℃;

[0064] A3. Add modified talcum powder, cetyltrimethylammonium chloride and polyglycerol alkyl ether, stir for 10 minutes at a temperature of 70°C, stir until no precipitation occurs, and obtain a rosin sizing agent;

[0065] A4. Heat and melt the strengthened rosin gum, and add trimethylolpropane in batches, with an interva...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention provides a rosin sizing agent and a preparation method thereof. The raw material formula includes components in parts by weight: 20-40 parts of cationic rosin glue; 8-12 parts of reinforced rosin glue; 5-15 parts of modified talcum powder 10-20 parts of cyclodextrin; 10-18 parts of cetyltrimethylammonium chloride; 3-6 parts of polyglycerol alkyl ether; 3-5 parts of chitosan; 3-aminopropyl trimethoxy 2-5 parts of base silane. The technical effect of the invention is: the rosin sizing agent prepared by the formula and the preparation process has a high adhesion rate, and has relatively high oil resistance and stability.

Description

technical field [0001] The invention belongs to the technical field of rosin sizing agent and preparation technology, and in particular relates to a rosin sizing agent and a preparation method. Background technique [0002] The sizing agent is divided into two categories: rosin type and non-rosin type. Rosin-type sizing agents mainly use rosin, mainly including rosin glue, reinforced rosin glue, paraffin rosin glue, and dispersed rosin glue. High free rosin gum. Non-rosin sizing agents mainly include paraffin latex, sodium stearate, polyvinyl alcohol, carboxymethyl cellulose, animal glue, casein, starch, synthetic gum, etc. Rosin type sizing agent is mainly used for internal sizing, non-rosin type sizing agent is mostly used for surface sizing, and non-rosin type sizing agent is also used as internal sizing agent for paper or cardboard with special requirements. [0003] Sizing refers to a method of treating paper or board. The purpose of paper sizing is to render the pa...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): D21H21/16D21H19/14D21H19/24D21H17/62D21H17/69D21H17/24D21H17/07D21H17/53D21H17/13
CPCD21H21/16D21H19/14D21H19/24D21H17/62D21H17/69D21H17/24D21H17/07D21H17/53D21H17/13
Inventor 卢志勇栾星星
Owner 浙江百斯特化工有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products