Lavender flavor type environment protective latex paint and its preparation method
An environmentally friendly latex and lavender technology, applied in latex paint, coating, etc., can solve problems such as single function and unsatisfactory
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment Construction
[0024] Weigh raw materials (kg) according to the following ratio:
[0025] Lavender essential oil 0.2, toilet water 14.4, styrene polyacrylic acid emulsion 16, titanium dioxide 17, kaolin 5.4, talcum powder 10, sodium hexametaphosphate 0.7, polyamide salt 0.3, water 36.
[0026] The production method is as follows:
[0027] 1. Add water, toilet water and lavender essential oil into the disperser, stir at 1200 rpm for 45 minutes, and add 1 / 3 of sodium hexametaphosphate during the stirring process;
[0028] 2. After stirring evenly, stop the machine for 30 minutes, then add titanium dioxide, kaolin, talcum powder and the remaining sodium hexametaphosphate, and start stirring at 800 rpm for 50 minutes;
[0029] 3. Add the homogenized material in step 2 into a sand mill, and grind for 120 minutes to obtain a finely ground slurry;
[0030] 4. Add the ground slurry into the disperser, stir at a speed of 360 rpm, add ammonia water, the amount of ammonia water added is 0.01-0.03% of...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com