A method for durable waterproof and wrinkle-resistant finishing of polyester/cotton dark twill lining cloth
A technology for anti-wrinkle finishing and lining cloth, applied in the field of textiles, can solve the problems of serious wrinkles, prolonged production process time, unsatisfactory effect, etc., and achieves the effect of soft fabric structure, remarkable non-iron effect, and excellent washing resistance.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] Take the polyester / cotton dark twill lining cloth and perform the following finishing process:
[0027] Pad resin water repellent (fluid rate 75%) → pre-drying → tentering drying, control the moisture content of 12% when dropping cloth) → friction calendering → wet stacking → baking (170℃, 5min) →Soaping→Water washing→Neutralization→Padding anti-wrinkle finishing liquid→rolling and outsourcing plastic film→room temperature stacking→relaxing→leaving for 6h→water washing→drying;
[0028] The composition of the resin water repellent finishing agent solution is as follows:
[0029] Melamine resin CHD4g / L
[0030] Catalyst 3g / L
[0031] Silicone waterproofing agent emulsion 6g / L
[0032] The pre-drying adopts heat to dry at 80°C to reduce the moisture content of the fabric to below 30%;
[0033] The stenter drying is performed on a heat distribution clip stenter;
[0034] The friction calendering process is carried out twice in sequence. The composition of the rollers is 2 soft rollers,...
Embodiment 2
[0043] Take the polyester / cotton dark twill lining cloth and perform the following finishing process
[0044] Dipping resin water repellent (fluid rate 85%) → pre-drying → tentering drying (controlling moisture content of 16% when dropping cloth) → friction calendering → wet stacking → baking (180°C, 4min) →Soaping→Water washing→Neutralization→Padding anti-wrinkle finishing liquid→rolling and outsourcing plastic film→room temperature stacking→relaxing→leaving for 8h→water washing→drying;
[0045] Wherein, the composition of the resin water repellent finishing agent solution:
[0046] Melamine resin CHD4g / L
[0047] Catalyst 6g / L
[0048] Water and oil repellent emulsion 4g / L
[0049] The pre-drying adopts heat separation or infrared ray drying at 100°C to reduce the moisture content of the fabric to below 30%;
[0050] The stenter drying is performed on a hot-air pin stenter;
[0051] The friction calendering process is carried out twice in sequence. The composition of the rollers is 2 so...